Find suppliers for this alloyC33000
Chemical Composition
Element
Cu(1)PbZnFe
(1) Cu + Sum of Named Elements 99.6% min.
Min (%)65.00.25
Max (%)68.00.7Rem0.07
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Cold Work
(%)
TubeHardH0475   Typ
60   Typ
7   Typ
80   Typ
69   Typ
35
Nominal Grain Size 0.025 mmOS02552   Typ
20   Typ
50   Typ
75   Typ
37   Typ
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
60   Typ
64   Typ
26   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1720
Melting Point - Solidus°F1660
Densitylb/cu in. at 68°F0.307
Specific Gravity8.5
Electrical Conductivity% IACS at 68°F26
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F67
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.2
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedPoor
Machinability Rating60
Common Fabrication Processes
  • Forming and Bending
  • Machining
  • Piercing and Punching
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001200
Typical uses
Product Category Product Reason Category Reason
IndustrialPower and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance
Power and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance to Fresh Water
Power and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance to Salt Water
Power and Pump Cylinder LinersMachining CharacteristicsMachinability
Power and Pump Cylinder LinersMechanical PropertiesDuctility
Power and Pump Cylinder LinersSolderabilitySolderability
Power and Pump Cylinder LinersWelding CharacteristicsWeldability
Power and Pump CylindersBrazing CharacteristicsBrazability
Power and Pump CylindersCorrosion ResistanceCorrosion Resistance
Power and Pump CylindersFinishing CharacteristicsPolishable
Power and Pump CylindersMachining CharacteristicsMachinability
Power and Pump CylindersMechanical PropertiesDuctility
Power and Pump CylindersSolderabilitySolderability
OrdnancePrimersCorrosion ResistanceCorrosion Resistance
PrimersForming CharacteristicsFormability
PrimersMachining CharacteristicsMachinability
PrimersMechanical PropertiesDuctility
PrimersMechanical PropertiesModerate Strength
PlumbingJ BendsCorrosion ResistanceCorrosion Resistance
J BendsCorrosion ResistanceCorrosion Resistance to Fresh Water
J BendsCorrosion ResistanceCorrosion Resistance to Salt Water
J BendsForming CharacteristicsFormability
J BendsMachining CharacteristicsMachinability
J BendsSolderabilitySolderability
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance to Fresh Water
Plumbing AccessoriesForming CharacteristicsFormability
Plumbing AccessoriesMachining CharacteristicsMachinability
Plumbing AccessoriesSolderabilitySolderability
Plumbing Brass GoodsCorrosion ResistanceCorrosion Resistance
Plumbing Brass GoodsCorrosion ResistanceCorrosion Resistance to Fresh Water
Plumbing Brass GoodsForming CharacteristicsFormability
Plumbing Brass GoodsMachining CharacteristicsMachinability
Plumbing Brass GoodsSolderabilitySolderability
Pump LinesCorrosion ResistanceCorrosion Resistance
Pump LinesCorrosion ResistanceCorrosion Resistance to Fresh Water
Pump LinesCorrosion ResistanceCorrosion Resistance to Salt Water
Pump LinesForming CharacteristicsFormability
Pump LinesMachining PropertiesMachinability, Good
Pump LinesSolderabilitySolderability
Trap LinesCorrosion ResistanceCorrosion Resistance
Trap LinesCorrosion ResistanceCorrosion Resistance to Fresh Water
Trap LinesCorrosion ResistanceCorrosion Resistance to Salt Water
Trap LinesForming CharacteristicsFormability
Trap LinesMachining PropertiesMachinability, Good
Trap LinesSolderabilitySolderability
Applicable Specifications
Form Sub-Form Specific Sub-Form System Standard Description
Seamless TubeASMESB135SEAMLESS BRASS TUBE
TubeSeamlessAMS4554BRASS TUBING, SEAMLESS, LIGHT ANNEALED
SeamlessAMS4555BRASS TUBING SEAMLESS, LIGHT ANNEALED
SeamlessASTMB135Tube, Seamless
Seamless (Metric)ASTMB135/B135MSeamless Brass Tube
SeamlessFEDERALWW-T-791TUBING: BRASS, SEAMLESS
SeamlessMILITARYMIL-T-46072TUBE, ROUND COPPER ALLOYS (LEADED BRASS), SEAMLESS
SeamlessSAEJ461WROUGHT AND CAST COPPER ALLOYS
SeamlessSAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.