Chemical Composition
Element
CuPbZnFe
Min (%)65.00.8
Max (%)68.01.5Rem0.06
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Cold Work
(%)
TubeHardH0475   Typ
60   Typ
7   Typ
80   Typ
69   Typ
35
Nominal Grain Size 0.025 mmOS02552   Typ
20   Typ
50   Typ
75   Typ
37   Typ
Nominal Grain Size 0.050 mmOS05047   Typ
15   Typ
60   Typ
64   Typ
26   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1720
Melting Point - Solidus°F1660
Densitylb/cu in. at 68°F0.307
Specific Gravity8.5
Electrical Conductivity% IACS at 68°F26
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F67
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.2
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedPoor
Machinability Rating60
Common Fabrication Processes
  • Forming and Bending
  • Machining
  • Piercing and Punching
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001200
Typical uses
Product Category Product Reason Category Reason
IndustrialPower and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance
Power and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance to Fresh Water
Power and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance to Petroleum Produsts
Power and Pump Cylinder LinersCorrosion ResistanceCorrosion Resistance to Salt Water
Power and Pump Cylinder LinersMachining CharacteristicsMachinability
Power and Pump Cylinder LinersMechanical PropertiesDuctility
Power and Pump Cylinder LinersSolderabilitySolderability
Power and Pump CylindersCorrosion ResistanceCorrosion Resistance
Power and Pump CylindersCorrosion ResistanceCorrosion Resistance to Fresh Water
Power and Pump CylindersCorrosion ResistanceCorrosion Resistance to Petroleum Produsts
Power and Pump CylindersCorrosion ResistanceCorrosion Resistance to Salt Water
Power and Pump CylindersMachining CharacteristicsMachinability
Power and Pump CylindersMechanical PropertiesDuctility
Power and Pump CylindersSolderabilitySolderability
OrdnancePrimersCorrosion ResistanceCorrosion Resistance
PrimersForming CharacteristicsFormability
PrimersMachining CharacteristicsMachinability
PrimersMechanical PropertiesDuctility
PrimersMechanical PropertiesModerate Strength
PlumbingPlumbing AccessoriesCorrosion ResistanceCorrosion Resistance
Plumbing AccessoriesCorrosion ResistanceCorrosion Resistance to Fresh Water
Plumbing AccessoriesMachining CharacteristicsMachinability
Plumbing AccessoriesMechanical PropertiesDuctility
Plumbing AccessoriesSolderabilitySolderability
Plumbing Brass GoodsCorrosion ResistanceCorrosion Resistance
Plumbing Brass GoodsCorrosion ResistanceCorrosion Resistance to Fresh Water
Plumbing Brass GoodsForming CharacteristicsFormability
Plumbing Brass GoodsMachining CharacteristicsMachinability
Plumbing Brass GoodsMechanical PropertiesDuctility
Plumbing Brass GoodsSolderabilitySolderability
Applicable Specifications
Form System Standard Description
TubeMILITARYMIL-T-46072TUBE, ROUND COPPER ALLOYS (LEADED BRASS), SEAMLESS
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS