C33200
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Pb | Zn | Fe | |
|
(1) Cu + Sum of Named Elements 99.6% min. |
||||
| Min (%) | 65.0 | 1.5 | ||
| Max (%) | 68.0 | 2.5 | Rem | 0.07 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Torsion Modulus (ksi) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||||
| Tube | Drawn General Purpose | H58 |
65 Typ |
50 Typ |
32 Typ |
|||||
| Hard | H04 |
75 Typ |
60 Typ |
7 Typ |
80 Typ |
69 Typ |
35 | |||
| Hard Drawn | H80 |
75 Typ |
60 Typ |
7 Typ |
5.7 Typ | |||||
| Nominal Grain Size 0.025 mm | OS025 |
52 Typ |
20 Typ |
50 Typ |
75 Typ |
37 Typ |
||||
| Nominal Grain Size 0.050 mm | OS050 |
47 Typ |
15 Typ |
60 Typ |
64 Typ |
26 Typ |
||||
| Melting Point - Liquidus°F | 1710 |
|---|---|
| Melting Point - Solidus°F | 1650 |
| Densitylb/cu in. at 68°F | 0.308 |
| Specific Gravity | 8.53 |
| Electrical Conductivity% IACS at 68°F | 26 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 67 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.3 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15000 |
| Modulus of Rigidityksi | 5600 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Fair |
| Seam Weld | Not Recommended |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Poor |
| Machinability Rating | 60 |
Common Fabrication Processes
- Forming and Bending
- Machining
- Piercing and Punching
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1200 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Hydraulic Controls | Corrosion Resistance | Corrosion Resistance |
| Hydraulic Controls | Machining Characteristics | Machinability | |
| Power and Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance | |
| Power and Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Power and Pump Cylinder Liners | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Power and Pump Cylinder Liners | Machining Characteristics | Machinability | |
| Power and Pump Cylinder Liners | Mechanical Properties | Moderate Strength | |
| Power and Pump Cylinder Liners | Solderability | Solderability | |
| Power and Pump Cylinders | Corrosion Resistance | Corrosion Resistance | |
| Power and Pump Cylinders | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Power and Pump Cylinders | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Power and Pump Cylinders | Machining Characteristics | Machinability | |
| Power and Pump Cylinders | Mechanical Properties | Moderate Strength | |
| Power and Pump Cylinders | Solderability | Solderability | |
| Screw Machine Products | Corrosion Resistance | Corrosion Resistance | |
| Screw Machine Products | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Screw Machine Products | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Screw Machine Products | Machining Characteristics | Machinability | |
| Screw Machine Products | Mechanical Properties | Moderate Strength | |
| Ordnance | Primers | Corrosion Resistance | Corrosion Resistance |
| Primers | Forming Characteristics | Formability | |
| Primers | Machining Characteristics | Machinability | |
| Primers | Mechanical Properties | Ductility | |
| Primers | Mechanical Properties | Moderate Strength | |
| Plumbing | Plumbing Accessories | Corrosion Resistance | Corrosion Resistance |
| Plumbing Accessories | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Plumbing Accessories | Forming Characteristics | Formability | |
| Plumbing Accessories | Machining Characteristics | Machinability | |
| Plumbing Accessories | Solderability | Solderability | |
| Plumbing Brass Goods | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Brass Goods | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Plumbing Brass Goods | Forming Characteristics | Formability | |
| Plumbing Brass Goods | Machining Characteristics | Machinability | |
| Plumbing Brass Goods | Solderability | Solderability |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Seamless Tube | ASME | SB135 | SEAMLESS BRASS TUBE | ||
| Tube | ASTM | B135 | Tube, Seamless | ||
| AMS | 4558 | BRASS TUBING, SEAMLESS DRAWN TEMPER | |||
| MILITARY | MIL-T-46072 | TUBE, ROUND COPPER ALLOYS (LEADED BRASS), SEAMLESS | |||
| Seamless (Metric) | ASTM | B135/B135M | Seamless Brass Tube |