C34900
| Elements | ||||
|---|---|---|---|---|
| Cu | Pb | Zn | Fe | |
| Min (%) | 61.0 | 0.10 | ||
| Max (%) | 64.0 | 0.50 | Rem | 0.10 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Torsion Modulus (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| Rod | Nominal Grain Size 0.035 mm | OS035 |
53 Typ |
24 Typ |
50 Typ |
5.7 Typ | 34 Typ |
0.24 |
| Rod & Wire | 1/4 Hard | H01 |
68 Typ |
55 Typ |
18 Typ |
41 Typ |
0.24 | |
| 1/4 Hard | H01 |
56 Typ |
42 Typ |
42 Typ |
36 Typ |
1 | ||
| Wire | Nominal Grain Size 0.015 mm | OS015 |
55 Typ |
22 Typ |
48 Typ |
35 Typ |
0.24 | |
| Nominal Grain Size 0.050 mm | OS050 |
48 Typ |
16 Typ |
72 Typ |
32 Typ |
0.75 | ||
Physical Properties
Fabrication Properties
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Builders Hardware | Hardware | Corrosion Resistance | Corrosion Resistance |
| Hardware | Forming Characteristics | Formability | |
| Hardware | Machining Characteristics | Excellent Machinability | |
| Fasteners | Rivets | Corrosion Resistance | Corrosion Resistance |
| Rivets | Forming Characteristics | Cold Workability | |
| Rivets | Forming Characteristics | Formability | |
| Rivets | Machining Characteristics | Excellent Machinability | |
| Saw Nuts | Corrosion Resistance | Corrosion Resistance | |
| Saw Nuts | Machining Characteristics | Excellent Machinability | |
| Saw Nuts | Mechanical Properties | Moderate Strength | |
| Plumbing | Plumbing goods | Corrosion Resistance | Corrosion Resistance |
| Plumbing goods | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Plumbing goods | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Plumbing goods | Forming Characteristics | Cold Workability | |
| Plumbing goods | Forming Characteristics | Formability | |
| Plumbing goods | Machining Characteristics | Excellent Machinability |
Applicable Specifications
Corrosion Properties