Find suppliers for this alloyC34900
Chemical Composition
Element
CuPbZnFe
Min (%)61.00.10
Max (%)64.00.50Rem0.10
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Torsion Modulus
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
RodNominal Grain Size 0.035 mmOS03553   Typ
24   Typ
50   Typ
5.7   Typ
34   Typ
0.24
Rod & Wire1/4 HardH0168   Typ
55   Typ
18   Typ
41   Typ
0.24
H0156   Typ
42   Typ
42   Typ
36   Typ
1
WireNominal Grain Size 0.015 mmOS01555   Typ
22   Typ
48   Typ
35   Typ
0.24
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
72   Typ
32   Typ
0.75
* Measured at room temperature, 68°F (20°C).
Physical Properties

No physical properties for this alloy

Fabrication Properties

No fabrication properties for this alloy

Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
Builders HardwareHardwareCorrosion ResistanceCorrosion Resistance
HardwareForming CharacteristicsFormability
HardwareMachining CharacteristicsExcellent Machinability
FastenersRivetsCorrosion ResistanceCorrosion Resistance
RivetsForming CharacteristicsCold Workability
RivetsForming CharacteristicsFormability
RivetsMachining CharacteristicsExcellent Machinability
Saw NutsCorrosion ResistanceCorrosion Resistance
Saw NutsMachining CharacteristicsExcellent Machinability
Saw NutsMechanical PropertiesModerate Strength
PlumbingPlumbing goodsCorrosion ResistanceCorrosion Resistance
Plumbing goodsCorrosion ResistanceCorrosion Resistance to Fresh Water
Plumbing goodsCorrosion ResistanceCorrosion Resistance to Salt Water
Plumbing goodsForming CharacteristicsCold Workability
Plumbing goodsForming CharacteristicsFormability
Plumbing goodsMachining CharacteristicsExcellent Machinability
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties