Find suppliers for this alloyC35000
Chemical Composition
Element
Cu(1,2)PbZnFe(3)
(1) Cu + Sum of Named Elements 99.6% min. (2) Cu, 61.0% min. for rod. (3) For flat products, the iron shall be 0.10% max.
Min (%)60.00.8
Max (%)63.02.0Rem0.15
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Flat Products1/2 HardH0260   Typ
45   Typ
45   Typ
29   Typ
66   Typ
60   Typ
0.04
1/4 HardH0154   Typ
34   Typ
32   Typ
43   Typ
53   Typ
52   Typ
0.04
3/4 HardH0367   Typ
55   Typ
53   Typ
17   Typ
75   Typ
68   Typ
0.04
Extra HardH0684   Typ
69   Typ
65   Typ
5   Typ
86   Typ
75   Typ
0.04
HardH0473   Typ
60   Typ
60   Typ
10   Typ
80   Typ
71   Typ
0.04
Nominal Grain Size 0.015 mmOS01551   Typ
25   Typ
25   Typ
46   Typ
74   Typ
0.04
Nominal Grain Size 0.025 mmOS02548   Typ
20   Typ
20   Typ
50   Typ
70   Typ
0.04
Nominal Grain Size 0.035 mmOS03547   Typ
16   Typ
16   Typ
54   Typ
67   Typ
0.04
Nominal Grain Size 0.050 mmOS05045   Typ
13   Typ
13   Typ
57   Typ
61   Typ
0.04
Flat Products & Rod1/2 HardH0270   Typ
52   Typ
22   Typ
42   Typ
0.47
H0260   Typ
45   Typ
29   Typ
0.04
1/4 HardH0158   Typ
44   Typ
42   Typ
38   Typ
0.47
H0154   Typ
34   Typ
43   Typ
0.04
Nominal Grain Size 0.015 mmOS01555   Typ
25   Typ
46   Typ
36   Typ
0.47
OS01551   Typ
25   Typ
46   Typ
0.04
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
56   Typ
34   Typ
0.47
OS05045   Typ
13   Typ
57   Typ
0.04
Rod1/2 HardH0255   Min for Standard
70   Max for Standard
25   Min for Standard
10   Min for Standard
80   Typ
70   Typ
42   Typ
0.75
H0250   Min for Standard
62   Max for Standard
20   Min for Standard
15   Min for Standard
5.7   Typ
1.375
H0257   Min for Standard
80   Max for Standard
25   Min for Standard
7   Min for Standard
<0.50
1/4 HardH0142   Min for Standard
62   Max for Standard
15   Min for Standard
20   Min for Standard
1.375
H0150   Min for Standard
62   Max for Standard
20   Min for Standard
15   Min for Standard
60   Typ
57   Typ
38   Typ
0.75
H0152   Min for Standard
65   Max for Standard
25   Min for Standard
10   Min for Standard
<0.50
Nominal Grain Size 0.015 mmOS01555   Typ
25   Typ
46   Typ
85   Typ
50   Typ
36   Typ
0.5
Nominal Grain Size 0.050 mmOS05048   Typ
16   Typ
56   Typ
65   Typ
25   Typ
34   Typ
0.5
Soft AnnealO6044   Min for Standard
15   Min for Standard
25   Min for Standard
0.75
O6040   Min for Standard
15   Min for Standard
30   Min for Standard
1.375
O6046   Min for Standard
16   Min for Standard
20   Min for Standard
<0.50
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1680
Melting Point - Solidus°F1640
Densitylb/cu in. at 68°F0.305
Specific Gravity8.44
Electrical Conductivity% IACS at 68°F26
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F67
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedFair
Capacity for Being Hot FormedFair
Forgeability Rating50
Machinability Rating70
Common Fabrication Processes
  • Blanking
  • Machining
  • Piercing and Punching
  • Roll Threading and Knurling
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001100
Hot Treatment14001500
Typical uses
Product Category Product Reason Category Reason
Builders HardwareHingesAppearanceAppearance
HingesCorrosion ResistanceCorrosion Resistance
HingesMachining CharacteristicsMachinability
HingesMechanical PropertiesModerate Strength
ConsumerKeysCorrosion ResistanceCorrosion Resistance
KeysMachining CharacteristicsMachinability
KeysMechanical PropertiesModerate Strength
Lock PartsCorrosion ResistanceCorrosion Resistance
Lock PartsMachining CharacteristicsMachinability
Lock PartsMechanical PropertiesModerate Strength
Lock TumblersCorrosion ResistanceCorrosion Resistance
Lock TumblersMachining CharacteristicsMachinability
Lock TumblersMechanical PropertiesModerate Strength
FastenersNutsCorrosion ResistanceCorrosion Resistance
NutsMachining CharacteristicsMachinability
NutsMechanical PropertiesModerate Strength
WashersCorrosion ResistanceCorrosion Resistance
WashersMachining CharacteristicsMachinability
WashersMechanical PropertiesModerate Strength
IndustrialBearing CagesCorrosion ResistanceCorrosion Resistance
Bearing CagesMachining CharacteristicsMachinability
Bearing CagesMechanical PropertiesModerate Strength
Book DiesCorrosion ResistanceCorrosion Resistance
Book DiesMachining CharacteristicsMachinability
Book DiesMechanical PropertiesModerate Strength
Clock PlatesAppearanceAppearance
Clock PlatesCorrosion ResistanceCorrosion Resistance
Clock PlatesMachining CharacteristicsMachinability
Clock PlatesMechanical PropertiesModerate Strength
Engraving PlatesAppearanceAppearance
Engraving PlatesCorrosion ResistanceCorrosion Resistance
Engraving PlatesMachining CharacteristicsMachinability
Engraving PlatesMechanical PropertiesModerate Strength
GearsCorrosion ResistanceCorrosion Resistance
GearsMachining CharacteristicsMachinability
GearsMechanical PropertiesModerate Strength
Hose CouplingsCorrosion ResistanceCorrosion Resistance
Hose CouplingsMachining CharacteristicsMachinability
Hose CouplingsMechanical PropertiesModerate Strength
Meter PartsCorrosion ResistanceCorrosion Resistance
Meter PartsMachining CharacteristicsMachinability
Meter PartsMechanical PropertiesModerate Strength
Strike PlatesAppearanceAppearance
Strike PlatesCorrosion ResistanceCorrosion Resistance
Strike PlatesMachining CharacteristicsMachinability
Strike PlatesMechanical PropertiesModerate Strength
TemplatesCorrosion ResistanceCorrosion Resistance
TemplatesMachining CharacteristicsMachinability
TemplatesMechanical PropertiesModerate Strength
Type CharactersCorrosion ResistanceCorrosion Resistance
Type CharactersMachining CharacteristicsMachinability
Type CharactersMechanical PropertiesModerate Strength
Wear PlatesCorrosion ResistanceCorrosion Resistance
Wear PlatesMachining CharacteristicsExcellent Machinability
Wear PlatesMechanical PropertiesModerate Strength
PlumbingSink StrainersCorrosion ResistanceCorrosion Resistance
Sink StrainersMachining CharacteristicsMachinability
Sink StrainersMechanical PropertiesModerate Strength
Applicable Specifications
Form System Standard Description
BarASTMB121/B121MLEADED BRASS PLATE, SHEET, STRIP AND ROLLED BAR
PlateASTMB121/B121MLEADED BRASS PLATE, SHEET, STRIP AND ROLLED BAR
RodSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Rod, Bar & ShapesASTMB453/B453MCOPPER-ZINC-LEAD ALLOY (LEADED-BRASS) ROD
SheetASTMB121/B121MLEADED BRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
StripASTMB121/B121MLEADED BRASS PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties