Find suppliers for this alloy
C35330
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Pb(2) | Zn | As | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Pb may be reduced to 1.0% by agreement. |
||||
| Min (%) | 59.5 | 1.5 | 0.02 | |
| Max (%) | 64.0 | 3.5 | Rem | 0.25 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Section Size (in) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| Rod & Wire | 1/2 Hard | H02 |
50 Typ |
35 Typ |
20 Typ |
40 Min 75 Max |
1/2 - 1 |
| 1/2 Hard | H02 |
45 Typ |
30 Typ |
30 Typ |
40 Min 65 Max |
1 - 2 | |
| 1/2 Hard | H02 |
55 Typ |
40 Typ |
10 Typ |
65 Min 85 Max |
=<1/2 | |
| 1/2 Hard | H02 |
40 Typ |
25 Typ |
35 Typ |
30 Min 55 Max |
>2 | |
| Soft Anneal | O60 |
40 Typ |
25 Typ |
25 Typ |
40 Min 70 Max |
=<1 | |
| Melting Point - Liquidus°F | 1660 |
|---|---|
| Melting Point - Solidus°F | 1645 |
| Densitylb/cu in. at 68°F | 0.305 |
| Specific Gravity | 8.45 |
| Electrical Conductivity% IACS at 68°F | 26 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 12.4 |
| Modulus of Elasticity in Tensionksi | 15000 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Plumbing | Plumbers' Brass Goods | Appearance | Appearance |
| Plumbers' Brass Goods | Corrosion Resistance | Dezincification Resistance | |
| Plumbers' Brass Goods | Machining Characteristics | Machinability | |
| Plumbers' Brass Goods | Solderability | Solderability | |
| Plumbing Fittings | Corrosion Resistance | Corrosion Resistance | |
| Plumbing Fittings | Forming Characteristics | Cold Workability | |
| Plumbing Fittings | Machining Characteristics | Machinability | |
| Plumbing Fittings | Mechanical Properties | Ductility - better than C35300 or C36000 |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Forgings, Die (Hot Pressed) | ASME | SB283 | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | ||
| ASTM | B283/B283M | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | |||
| Rod, Bar & Shapes | Forgings | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | |
| ASTM | B453/B453M | COPPER-ZINC-LEAD ALLOY (LEADED-BRASS) ROD |
Corrosion Properties