Find suppliers for this alloyC35330
Chemical Composition
Element
Cu(1)Pb(2)ZnAs
(1) Cu + Sum of Named Elements 99.5% min. (2) Pb may be reduced to 1.0% by agreement.
Min (%)59.51.50.02
Max (%)64.03.5Rem0.25
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Section Size
(in)
Rod & Wire1/2 HardH0250   Typ
35   Typ
20   Typ
40   Min
75   Max
1/2 - 1
H0245   Typ
30   Typ
30   Typ
40   Min
65   Max
1 - 2
H0255   Typ
40   Typ
10   Typ
65   Min
85   Max
=<1/2
H0240   Typ
25   Typ
35   Typ
30   Min
55   Max
>2
Soft AnnealO6040   Typ
25   Typ
25   Typ
40   Min
70   Max
=<1
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1660
Melting Point - Solidus°F1645
Densitylb/cu in. at 68°F8.45
Specific Gravity8.45
Electrical Conductivity% IACS at 68°F26
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)12.4
Modulus of Elasticity in Tensionksi15000
Fabrication Properties

No fabrication properties for this alloy

Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
PlumbingPlumbers' Brass GoodsAppearanceAppearance
Plumbers' Brass GoodsCorrosion ResistanceDezincification Resistance
Plumbers' Brass GoodsMachining CharacteristicsMachinability
Plumbers' Brass GoodsSolderabilitySolderability
Plumbing FittingsCorrosion ResistanceCorrosion Resistance
Plumbing FittingsForming CharacteristicsCold Workability
Plumbing FittingsMachining CharacteristicsMachinability
Plumbing FittingsMechanical PropertiesDuctility - better than C35300 or C36000
Applicable Specifications
Form Sub-Form System Standard Description
Forgings, Die (Hot Pressed)ASMESB283COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
ASTMB283/B283MCOPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
Rod, Bar & ShapesForgingsASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
ASTMB453/B453MCOPPER-ZINC-LEAD ALLOY (LEADED-BRASS) ROD
Corrosion Properties

No information available.