Find suppliers for this alloyC36500
Chemical Composition
Element
Cu(1)PbSnZnFe
(1) Cu + Sum of Named Elements 99.6% min.
Min (%)58.00.25
Max (%)61.00.70.25Rem0.15
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell F scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Section Size
(in)
PlateAs Hot RolledM2054   Typ
20   Typ
45   Typ
80   Typ
40   Typ
5.7   Typ
1
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1650
Melting Point - Solidus°F1630
Densitylb/cu in. at 68°F0.304
Specific Gravity8.41
Electrical Conductivity% IACS at 68°F28
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F71
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.6
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedFair
Capacity for Being Hot FormedExcellent
Machinability Rating60
Common Fabrication Processes
  • Machining
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001100
Hot Treatment11501450
Typical uses
Product Category Product Reason Category Reason
ConsumerKey BlanksCorrosion ResistanceCorrosion Resistance
Key BlanksForging CharacteristicsForgability
Key BlanksMachining CharacteristicsMachinability
Key BlanksMechanical PropertiesModerate Strength
IndustrialCondenser TubeCorrosion ResistanceCorrosion Resistance
Condenser TubeCorrosion ResistanceCorrosion Resistance to Fresh Water
Condenser TubeCorrosion ResistanceCorrosion Resistance to Salt Water
Condenser TubeMachining CharacteristicsMachinability
Condenser Tube PlatesConductivity (Thermal)Thermal Conductivity
Condenser Tube PlatesCorrosion ResistanceCorrosion Resistance
Condenser Tube PlatesMachining CharacteristicsMachinability
Condenser Tube PlatesMechanical PropertiesModerate Strength
Engraving PlatesAppearanceAppearance
Engraving PlatesCorrosion ResistanceCorrosion Resistance
Engraving PlatesMachining CharacteristicsMachinability
Engraving PlatesMechanical PropertiesModerate Strength
Heat Exchanger BafflesConductivity (Thermal)Thermal Conductivity
Heat Exchanger BafflesCorrosion ResistanceCorrosion Resistance
Heat Exchanger BafflesMachining CharacteristicsMachinability
Heat Exchanger BafflesMechanical PropertiesModerate to High Strength
Heat Exchanger PlatesConductivity (Thermal)Thermal Conductivity
Heat Exchanger PlatesCorrosion ResistanceCorrosion Resistance
Heat Exchanger PlatesMachining CharacteristicsMachinability
Heat Exchanger PlatesMechanical PropertiesModerate High Strength
Support SheetsCorrosion ResistanceCorrosion Resistance
Support SheetsMachining CharacteristicsMachinability
Support SheetsMechanical PropertiesModerate Strength
OtherMain Tube Sheets for Condensers and Heat ExchangersCorrosion ResistanceCorrosion Resistance
Main Tube Sheets for Condensers and Heat ExchangersCorrosion ResistanceCorrosion Resistance to Fresh Water
Main Tube Sheets for Condensers and Heat ExchangersMachining CharacteristicsMachinability
Applicable Specifications
Form Sub-Form Specific Sub-Form Application System Standard Description
BarASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
Forgings, Die (Hot Pressed)ASMESB283COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
ASTMB283/B283MCOPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
PlateCladASTMB432COPPER AND COPPER ALLOY CLAD STEEL PLATE
Plate & Sheet for Pressure Vessels, Condensers & Heat ExchangersCondenser TubeASMESB171COPPER ALLOY CONDENSER TUBE PLATES
for Pressure Vessels, Condensers & Heat ExchangersCondenser TubeASTMB171/B171MCOPPER ALLOY CONDENSER TUBE PLATES
RodForgingsASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
Rod, Bar & ShapesASTMB981/B981MLOW LEADED BRASS ROD, BAR AND SHAPES
ShapesForgingsASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
Corrosion Properties

No information available.