Find suppliers for this alloyC36800
Chemical Composition
Element
CuPbSnZnFeP
Min (%)58.00.250.02
Max (%)61.00.70.25Rem0.150.10
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell F scale
Shear Strength
(ksi)
Section Size
(in)
PlateAs Hot RolledM2054   Typ
20   Typ
45   Typ
80   Typ
40   Typ
1
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1650
Melting Point - Solidus°F1630
Densitylb/cu in. at 68°F0.304
Specific Gravity8.41
Electrical Conductivity% IACS at 68°F28
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F71
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11.6
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedFair
Capacity for Being Hot FormedExcellent
Machinability Rating60
Common Fabrication Processes
  • Machining
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001100
Hot Treatment11501450
Typical uses
Product Category Product Reason Category Reason
IndustrialCondenser Tube PlatesConductivity (Thermal)Thermal Conductivity
Condenser Tube PlatesCorrosion ResistanceCorrosion Resistance
Condenser Tube PlatesCorrosion ResistanceCorrosion Resistance to Fresh Water
Condenser Tube PlatesCorrosion ResistanceCorrosion Resistance to Salt Water
Condenser Tube PlatesMachining CharacteristicsMachinability
Condenser Tube PlatesMechanical PropertiesModerate Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.