Find suppliers for this alloy
C40410
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
|||||
| Min (%) | 95.0 | 0.1 | |||
| Max (%) | 99.0 | 0.05 | 0.40 | Rem | 0.05 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||
| Flat Products | Hard | H04 |
59.5 Min 72.5 Typ 89.9 Max |
58 Min 71.1 Typ 88.5 Max |
| Melting Point - Liquidus°F | 1926 |
|---|---|
| Melting Point - Solidus°F | 1899 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.81 |
| Electrical Conductivity% IACS at 68°F | 60 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 139.8 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17100 |
| Magnetic Permeability | 1 |
| Poisson's Ratio | 0.33 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Spot Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties