Find suppliers for this alloyC40800
Chemical Composition
Element
CuPbSnZnFe
Min (%)94.01.8
Max (%)96.00.052.2Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Flat Products1/2 HardH0254   Typ
55   Typ
46   Typ
12   Typ
65   Typ
62   Typ
38   Typ
0.04
1/4 HardH0150   Typ
39   Typ
24   Typ
36   Typ
0.04
H0150   Typ
45   Typ
39   Typ
24   Typ
50   Typ
54   Typ
36   Typ
0.04
3/4 HardH0362   Typ
60   Typ
52   Typ
6   Typ
72   Typ
67   Typ
41   Typ
0.04
Extra HardH0673   Typ
78   Typ
61   Typ
4   Typ
82   Typ
73   Typ
45   Typ
0.04
Extra SpringH1079   Typ
84   Typ
75   Typ
3   Typ
84   Typ
75   Typ
49   Typ
0.04
HardH0467   Typ
57   Typ
5   Typ
43   Typ
0.04
H0467   Typ
70   Typ
57   Typ
5   Typ
76   Typ
70   Typ
43   Typ
0.04
Nominal Grain Size 0.015 mmOS01545   Typ
15   Typ
42   Typ
69   Typ
31   Typ
34   Typ
0.04
Nominal Grain Size 0.025 mmOS02544   Typ
14   Typ
43   Typ
65   Typ
26   Typ
34   Typ
0.04
Nominal Grain Size 0.035 mmOS03542   Typ
13   Typ
43   Typ
33   Typ
0.04
OS03542   Typ
13   Typ
43   Typ
60   Typ
22   Typ
33   Typ
0.04
SpringH0879   Typ
66   Typ
3   Typ
48   Typ
0.04
H0879   Typ
82   Typ
66   Typ
3   Typ
85   Typ
77   Typ
48   Typ
6   Typ
0.04
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) For hard alloys.
(2) For annealed alloys.
Melting Point - Liquidus°F1930
Melting Point - Solidus°F1900
Densitylb/cu in. at 68°F0.32
Electrical Conductivity% IACS at 68°F37
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F92
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)10.1
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000(1)
Modulus of Elasticity in Tensionksi18000(2)
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedFair
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Shearing
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8501250
Hot Treatment15251635
Typical uses
Product Category Product Reason Category Reason
ArchitectureWeather StrippingAppearanceAppearance
Weather StrippingCorrosion ResistanceCorrosion Resistance
Weather StrippingMechanical PropertiesModerate Strength
Builders HardwareHardware, StampedAppearanceAppearance
Hardware, StampedCorrosion ResistanceCorrosion Resistance
Hardware, StampedForming CharacteristicsFormability
Hardware, StampedMechanical PropertiesModerate Strength
ConsumerCostume JewelryAppearanceAppearance
Costume JewelryCorrosion ResistanceCorrosion Resistance
Costume JewelryForming CharacteristicsFormability
Costume JewelryMechanical PropertiesModerate Strength
Costume JewelrySolderabilitySolderability
ElectricalConnectorsConductivity (Electrical)Electrical Conductivity
ConnectorsConductivity (Thermal)Thermal Conductivity
ConnectorsCorrosion ResistanceCorrosion Resistance
ConnectorsForming CharacteristicsFormability
ConnectorsMechanical PropertiesModerate Strength
IndustrialBushingsCorrosion ResistanceCorrosion Resistance
BushingsForming CharacteristicsFormability
BushingsFriction & Wear PropertiesWear Resistance
BushingsMechanical PropertiesModerate Strength
BushingsThermal PropertiesResistance to Stress Relaxation
Thrust WashersCorrosion ResistanceCorrosion Resistance
Thrust WashersForming CharacteristicsFormability
Thrust WashersFriction & Wear PropertiesWear Resistance
Thrust WashersMechanical PropertiesModerate Strength
Thrust WashersThermal PropertiesResistance to Stress Relaxation
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.