Find suppliers for this alloyC40850
Chemical Composition
Element
Cu(1)PbSnZnFePNi
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)94.52.60.050.010.05
Max (%)96.50.054.0Rem0.200.200.20
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Flat Products1/2 HardH0265   Typ
52   Typ
12   Typ
1/4 HardH0160   Typ
42   Typ
24   Typ
Extra HardH0694   Typ
91   Typ
4   Typ
HardH0481   Typ
76   Typ
6   Typ
Nominal Grain Size 0.015 mmOS01554   Typ
30   Typ
42   Typ
SpringH0898   Typ
96   Typ
3   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1940
Melting Point - Solidus°F1890
Densitylb/cu in. at 68°F0.32
Specific Gravity8.86
Electrical Conductivity% IACS at 68°F30
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F75
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)10.1
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingGood
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedFair
Machinability Rating20
Fabrication Process Properties

No fabrication process properties for this alloy

    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing6601350
Typical uses
Product Category Product Reason Category Reason
AutomotiveTerminals, automotiveConductivity (Electrical)Electrical Conductivity
Terminals, automotiveMechanical PropertiesDuctility
Terminals, automotiveMechanical PropertiesStrength
ElectricalConnectors, electronicConductivity (Electrical)Electrical Conductivity
Connectors, electronicCorrosion ResistanceStress Corrosion Crack Resistant
Connectors, electronicMechanical PropertiesStrength, Moderate
Connectors, electronicStress RelaxationStress Relaxation Resistance
Contact springsConductivity (Electrical)Electrical Conductivity
Contact springsCorrosion ResistanceCorrosion Resistance
Contact springsMechanical PropertiesModerate to High Strength
Contact springsSolderabilitySolderability
Lead FramesConductivity (Electrical)Electrical Conductivity
Applicable Specifications
Form Specific Sub-Form System Standard Description
BarASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
StripASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Electric Connector & Spring ContactASTMB888/B88MCOPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS
Corrosion Properties

No information available.