									C41100 
									
								
								
									
									
										
							  
							    
							
							  
							    
							
							  
							    
							
							  
							    
							
							  
								    
							
							  
							    
							
							  
							    
							
								
									
	| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | |
| (1) Cu + Sum of Named Elements  99.7% min. | |||||
| Min (%) | 89.0 | 0.30 | |||
| Max (%) | 92.0 | 0.09 | 0.7 | Rem | 0.05 | 
| Form | Temper | Temper Code | Tensile Strength (ksi) | YS-0.2% Offset (ksi) | YS-0.5% Ext (ksi) | Elongation (%) | Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) | Torsion Modulus (ksi) | Ultimate Tensile Strength in Shear (ksi) | Section Size (in) | Cold Work (%) | 
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||||||||
| Flat Products | 1/2 Hard | H02 | 55 Typ | 53 Typ | 47 Typ | 14 Typ | 61 Typ | 58 Typ | 36 Typ | 0.04 | ||||
| 1/4 Hard | H01 | 48 Typ | 41 Typ | 38 Typ | 23 Typ | 50 Typ | 51 Typ | 0.04 | ||||||
| 3/4 Hard | H03 | 60 Typ | 58 Typ | 52 Typ | 6 Typ | 70 Typ | 64 Typ | 0.04 | ||||||
| Extra Hard | H06 | 72 Typ | 70 Typ | 60 Typ | 4 Typ | 79 Typ | 69 Typ | 0.04 | ||||||
| Extra Spring | H10 | 80 Typ | 76 Typ | 2 Typ | 0.04 | |||||||||
| Extra Spring | H10 | 78 Typ | 76 Typ | 72 Typ | 2 Typ | 83 Typ | 71 Typ | 0.04 | ||||||
| Hard | H04 | 66 Typ | 64 Typ | 5 Typ | 40 Typ | 0.04 | ||||||||
| Hard | H04 | 66 Typ | 64 Typ | 55 Typ | 5 Typ | 75 Typ | 67 Typ | 40 Typ | 6.7 Typ | 0.04 | ||||
| Nominal Grain Size 0.015 mm | OS015 | 42 Typ | 15 Typ | 40 Typ | 34 Typ | 0.04 | ||||||||
| Nominal Grain Size 0.015 mm | OS015 | 42 Typ | 15 Typ | 12 Typ | 40 Typ | 69 Typ | 33 Typ | 34 Typ | 0.04 | |||||
| Nominal Grain Size 0.025 mm | OS025 | 41 Typ | 14 Typ | 12 Typ | 41 Typ | 66 Typ | 27 Typ | 0.04 | ||||||
| Nominal Grain Size 0.035 mm | OS035 | 39 Typ | 12 Typ | 11 Typ | 43 Typ | 60 Typ | 21 Typ | 33 Typ | 0.04 | |||||
| Nominal Grain Size 0.050 mm | OS050 | 38 Typ | 8.992 Typ | 44 Typ | 32 Typ | 0.04 | ||||||||
| Spring | H08 | 78 Typ | 75 Typ | 70 Typ | 3 Typ | 82 Typ | 71 Typ | 0.04 | ||||||
| Wire | Hard | H04 | 102 Typ | 1 Typ | 0.1 | 95 | ||||||||
| Hard | H04 | 106 Typ | 9 Typ | 0.05 | 98.7 | |||||||||
| Hard | H04 | 81 Typ | 2 Typ | 0.25 | 70 | |||||||||
| (1)For annealed alloys. | |
| Melting Point - Liquidus°F | 1905 | 
|---|---|
| Melting Point - Solidus°F | 1870 | 
| Densitylb/cu in. at 68°F | 0.318 | 
| Specific Gravity | 8.8 | 
| Electrical Conductivity% IACS at 68°F | 32 | 
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 75 | 
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10.2 | 
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 | 
| Modulus of Elasticity in Tensionksi | 18000 (1) | 
| Modulus of Rigidityksi | 6700 | 
| Technique | Suitability | 
|---|---|
| Soldering | Excellent | 
| Brazing | Excellent | 
| Oxyacetylene Welding | Fair | 
| Gas Shielded Arc Welding | Good | 
| Coated Metal Arc Welding | Not Recommended | 
| Spot Weld | Fair | 
| Seam Weld | Not Recommended | 
| Butt Weld | Good | 
| Capacity for Being Cold Worked | Excellent | 
| Capacity for Being Hot Formed | Good | 
| Machinability Rating | 20 | 
							  Common Fabrication Processes
- Blanking
- Drawing
- Forming and Bending
- Piercing and Punching
- Shearing
- Spinning
- Stamping
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 930 | 1290 | ||
| Hot Working Temperature | 1525 | 1635 | ||
| Product Category | Product | Reason Category | Reason | 
|---|---|---|---|
| Electrical | Conductors | Conductivity (Electrical) | Electrical Conductivity | 
| Conductors | Conductivity (Thermal) | Thermal Conductivity | |
| Conductors | Corrosion Resistance | Corrosion Resistance | |
| Conductors | Forming Characteristics | Formability | |
| Conductors | Mechanical Properties | Moderate Strength | |
| Conductors | Thermal Properties | Resistance to Stress Relaxation | |
| Electrical Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Electrical Connectors | Forming Characteristics | Formability | |
| Electrical Connectors | Mechanical Properties | Moderate Strength | |
| Fuse Clips | Conductivity (Electrical) | Electrical Conductivity | |
| Fuse Clips | Corrosion Resistance | Corrosion Resistance | |
| Fuse Clips | Forming Characteristics | Formability | |
| Fuse Clips | Mechanical Properties | Moderate Strength | |
| Fuse Clips | Thermal Properties | Resistance to Stress Relaxation | |
| Terminals | Conductivity (Electrical) | Electrical Conductivity | |
| Terminals | Conductivity (Thermal) | Thermal Conductivity | |
| Terminals | Corrosion Resistance | Corrosion Resistance | |
| Terminals | Forming Characteristics | Formability | |
| Terminals | Mechanical Properties | Moderate Strength | |
| Terminals | Thermal Properties | Resistance to Stress Relaxation | |
| Industrial | Bearing Sleeves | Corrosion Resistance | Corrosion Resistance | 
| Bearing Sleeves | Forming Characteristics | Formability | |
| Bearing Sleeves | Friction & Wear Properties | Wear Resistance | |
| Bearing Sleeves | Mechanical Properties | Moderate Strength | |
| Bearing Sleeves | Thermal Properties | Resistance to Stress Relaxation | |
| Bearings | Corrosion Resistance | Corrosion Resistance | |
| Bearings | Forming Characteristics | Formability | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Mechanical Properties | Moderate Strength | |
| Bearings | Thermal Properties | Resistance to Stress Relaxation | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Forming Characteristics | Formability | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | Moderate Strength | |
| Bushings | Thermal Properties | Resistance to Stress Relaxation | |
| Flexible Hose | Corrosion Resistance | Corrosion Resistance | |
| Flexible Hose | Forming Characteristics | Formability | |
| Flexible Hose | Mechanical Properties | Moderate Strength | |
| Flexible Hose | Thermal Properties | Resistance to Stress Relaxation | |
| Thrust Washers | Corrosion Resistance | Corrosion Resistance | |
| Thrust Washers | Forming Characteristics | Formability | |
| Thrust Washers | Friction & Wear Properties | Wear Resistance | |
| Thrust Washers | Mechanical Properties | Moderate Strength | |
| Thrust Washers | Thermal Properties | Resistance to Stress Relaxation | 
| Form | Specific Sub-Form | Application | System | Standard | Description | 
|---|---|---|---|---|---|
| Bar | ASTM | B591 | COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Bearings & Busings | MILITARY | MIL-B-13501 | BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED | ||
| Bushing Stock | MILITARY | MIL-B-13501 | BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED | ||
| Plate | ASTM | B591 | COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Sheet | ASTM | B591 | COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Strip | Flexible Hose | ASTM | B508 | COPPER ALLOY STRIP FOR FLEXIBLE METAL HOSE | |
| ASTM | B591 | COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR | 
								Corrosion Properties