Find suppliers for this alloyC41100
Chemical Composition
Element
Cu(1)PbSnZnFe
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)89.00.30
Max (%)92.00.090.7Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Ultimate Tensile Strength in Shear
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0255   Typ
53   Typ
47   Typ
14   Typ
61   Typ
58   Typ
36   Typ
0.04
1/4 HardH0148   Typ
41   Typ
38   Typ
23   Typ
50   Typ
51   Typ
0.04
3/4 HardH0360   Typ
58   Typ
52   Typ
6   Typ
70   Typ
64   Typ
0.04
Extra HardH0672   Typ
70   Typ
60   Typ
4   Typ
79   Typ
69   Typ
0.04
Extra SpringH1080   Typ
76   Typ
2   Typ
0.04
H1078   Typ
76   Typ
72   Typ
2   Typ
83   Typ
71   Typ
0.04
HardH0466   Typ
64   Typ
5   Typ
40   Typ
0.04
H0466   Typ
64   Typ
55   Typ
5   Typ
75   Typ
67   Typ
40   Typ
6.7   Typ
0.04
Nominal Grain Size 0.015 mmOS01542   Typ
15   Typ
40   Typ
34   Typ
0.04
OS01542   Typ
15   Typ
12   Typ
40   Typ
69   Typ
33   Typ
34   Typ
0.04
Nominal Grain Size 0.025 mmOS02541   Typ
14   Typ
12   Typ
41   Typ
66   Typ
27   Typ
0.04
Nominal Grain Size 0.035 mmOS03539   Typ
12   Typ
11   Typ
43   Typ
60   Typ
21   Typ
33   Typ
0.04
Nominal Grain Size 0.050 mmOS05038   Typ
8.992   Typ
44   Typ
32   Typ
0.04
SpringH0878   Typ
75   Typ
70   Typ
3   Typ
82   Typ
71   Typ
0.04
WireHardH04102   Typ
1   Typ
0.195
H04106   Typ
9   Typ
0.0598.7
H0481   Typ
2   Typ
0.2570
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) For annealed alloys.
Melting Point - Liquidus°F1905
Melting Point - Solidus°F1870
Densitylb/cu in. at 68°F0.318
Specific Gravity8.8
Electrical Conductivity% IACS at 68°F32
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F75
Coefficient of Thermal Expansion 68-21210⁻⁶ per °F (68 – 212°F)10.2
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi18000(1)
Modulus of Rigidityksi6700
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedGood
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Drawing
  • Forming and Bending
  • Piercing and Punching
  • Shearing
  • Spinning
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing9301290
Hot Treatment15251635
Typical uses
Product Category Product Reason Category Reason
ElectricalConductorsConductivity (Electrical)Electrical Conductivity
ConductorsConductivity (Thermal)Thermal Conductivity
ConductorsCorrosion ResistanceCorrosion Resistance
ConductorsForming CharacteristicsFormability
ConductorsMechanical PropertiesModerate Strength
ConductorsThermal PropertiesResistance to Stress Relaxation
Electrical ConnectorsConductivity (Electrical)Electrical Conductivity
Electrical ConnectorsForming CharacteristicsFormability
Electrical ConnectorsMechanical PropertiesModerate Strength
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsForming CharacteristicsFormability
Fuse ClipsMechanical PropertiesModerate Strength
Fuse ClipsThermal PropertiesResistance to Stress Relaxation
TerminalsConductivity (Electrical)Electrical Conductivity
TerminalsConductivity (Thermal)Thermal Conductivity
TerminalsCorrosion ResistanceCorrosion Resistance
TerminalsForming CharacteristicsFormability
TerminalsMechanical PropertiesModerate Strength
TerminalsThermal PropertiesResistance to Stress Relaxation
IndustrialBearing SleevesCorrosion ResistanceCorrosion Resistance
Bearing SleevesForming CharacteristicsFormability
Bearing SleevesFriction & Wear PropertiesWear Resistance
Bearing SleevesMechanical PropertiesModerate Strength
Bearing SleevesThermal PropertiesResistance to Stress Relaxation
BearingsCorrosion ResistanceCorrosion Resistance
BearingsForming CharacteristicsFormability
BearingsFriction & Wear PropertiesWear Resistance
BearingsMechanical PropertiesModerate Strength
BearingsThermal PropertiesResistance to Stress Relaxation
BushingsCorrosion ResistanceCorrosion Resistance
BushingsForming CharacteristicsFormability
BushingsFriction & Wear PropertiesWear Resistance
BushingsMechanical PropertiesModerate Strength
BushingsThermal PropertiesResistance to Stress Relaxation
Flexible HoseCorrosion ResistanceCorrosion Resistance
Flexible HoseForming CharacteristicsFormability
Flexible HoseMechanical PropertiesModerate Strength
Flexible HoseThermal PropertiesResistance to Stress Relaxation
Thrust WashersCorrosion ResistanceCorrosion Resistance
Thrust WashersForming CharacteristicsFormability
Thrust WashersFriction & Wear PropertiesWear Resistance
Thrust WashersMechanical PropertiesModerate Strength
Thrust WashersThermal PropertiesResistance to Stress Relaxation
Applicable Specifications
Form Application System Standard Description
BarASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Bearings & BusingsMILITARYMIL-B-13501BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED
Bushing StockMILITARYMIL-B-13501BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED
PlateASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
SheetASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
StripFlexible HoseASTMB508COPPER ALLOY STRIP FOR FLEXIBLE METAL HOSE
ASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Corrosion Properties

No information available.