C41120
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni | |
|
(1) Cu + Sum of Named Elements 99.7% min. |
|||||||
| Min (%) | 89.0 | 0.30 | 0.05 | 0.01 | 0.05 | ||
| Max (%) | 92.0 | 0.05 | 0.7 | Rem | 0.20 | 0.35 | 0.20 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Flat Products | 1/2 Hard | H02 |
67 Typ |
60 Typ |
12 Typ |
| 1/4 Hard | H01 |
60 Typ |
40 Typ |
24 Typ |
|
| Extra Hard | H06 |
84 Typ |
81 Typ |
5 Typ |
|
| Hard | H04 |
78 Typ |
73 Typ |
8 Typ |
|
| Nominal Grain Size 0.015 mm | OS015 |
54 Typ |
30 Typ |
40 Typ |
|
| Spring | H08 |
89 Typ |
85 Typ |
4 Typ |
|
| Melting Point - Liquidus°F | 1905 |
|---|---|
| Melting Point - Solidus°F | 1870 |
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.8 |
| Electrical Conductivity% IACS at 68°F | 40 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 100 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6700 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Fair |
| Seam Weld | Not Recommended |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 20 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 660 | 1350 | ||
Typical Uses
Applicable Specifications
Corrosion Properties