Find suppliers for this alloyC41300
Chemical Composition
Element
Cu(1)PbSnZnFe
(1) Cu + Sum of Named Elements 99.7% min.
Min (%)89.00.7
Max (%)93.00.091.3Rem0.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Shear Strength
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0256   Typ
50   Typ
17   Typ
68   Typ
64   Typ
39   Typ
0.04
1/4 HardH0149   Typ
40   Typ
29   Typ
53   Typ
54   Typ
36   Typ
0.04
3/4 HardH0364   Typ
55   Typ
6   Typ
76   Typ
70   Typ
42   Typ
0.04
Extra HardH0674   Typ
65   Typ
4   Typ
82   Typ
74   Typ
46   Typ
0.04
Extra SpringH1084   Typ
75   Typ
2   Typ
88   Typ
77   Typ
49   Typ
0.04
HardH0471   Typ
62   Typ
4   Typ
79   Typ
72   Typ
44   Typ
0.04
Nominal Grain Size 0.015 mmOS01546   Typ
17   Typ
40   Typ
63   Typ
25   Typ
35   Typ
0.04
Nominal Grain Size 0.025 mmOS02545   Typ
16   Typ
41   Typ
62   Typ
22   Typ
34   Typ
0.04
Nominal Grain Size 0.035 mmOS03544   Typ
16   Typ
42   Typ
61   Typ
21   Typ
34   Typ
0.04
Nominal Grain Size 0.050 mmOS05043   Typ
15   Typ
43   Typ
60   Typ
20   Typ
33   Typ
0.04
Nominal Grain Size 0.070 mmOS07042   Typ
12   Typ
44   Typ
58   Typ
18   Typ
32   Typ
0.04
Nominal Grain Size 0.100 mmOS10041   Typ
12   Typ
44   Typ
58   Typ
18   Typ
32   Typ
0.04
SpringH0879   Typ
70   Typ
3   Typ
86   Typ
76   Typ
48   Typ
0.04
Rod1/2 HardH0265   Typ
56   Typ
12   Typ
76   Typ
70   Typ
42   Typ
0.520
1/8 HardH0050   Typ
41   Typ
28   Typ
53   Typ
54   Typ
40   Typ
0.56
HardH0474   Typ
65   Typ
6   Typ
82   Typ
74   Typ
44   Typ
0.535
Nominal Grain Size 0.015 mmOS01548   Typ
22   Typ
42   Typ
64   Typ
24   Typ
39   Typ
0.5
Nominal Grain Size 0.050 mmOS05044   Typ
18   Typ
45   Typ
60   Typ
20   Typ
34   Typ
0.5
Wire1/2 HardH0267   Typ
58   Typ
10   Typ
42   Typ
0.08
1/4 HardH0155   Typ
44   Typ
18   Typ
39   Typ
0.08
1/8 HardH0047   Typ
37   Typ
30   Typ
38   Typ
0.08
3/4 HardH0376   Typ
72   Typ
6   Typ
46   Typ
0.08
Extra HardH0696   Typ
80   Typ
4   Typ
56   Typ
0.08
HardH0486   Typ
77   Typ
5   Typ
51   Typ
0.08
Nominal Grain Size 0.015 mmOS01547   Typ
21   Typ
41   Typ
36   Typ
0.08
Nominal Grain Size 0.025 mmOS02546   Typ
20   Typ
42   Typ
36   Typ
0.08
Nominal Grain Size 0.035 mmOS03545   Typ
18   Typ
43   Typ
35   Typ
0.08
Nominal Grain Size 0.050 mmOS05044   Typ
17   Typ
44   Typ
34   Typ
0.08
Nominal Grain Size 0.070 mmOS07043   Typ
16   Typ
45   Typ
33   Typ
0.08
SpringH08105   Typ
82   Typ
3   Typ
58   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1900
Melting Point - Solidus°F1850
Densitylb/cu in. at 68°F0.318
Specific Gravity8.8
Electrical Conductivity% IACS at 68°F30
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F77
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)10.3
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldFair
Seam WeldNot Recommended
Butt WeldGood
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedGood
Forgeability Rating50
Machinability Rating20
Common Fabrication Processes
  • Bending
  • Blanking
  • Coining
  • Drawing
  • Forming
  • Spinning
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing9001400
Hot Treatment14151460
Typical uses
Product Category Product Reason Category Reason
Builders HardwareHardwareAppearanceAppearance
HardwareCorrosion ResistanceCorrosion Resistance
HardwareForming CharacteristicsFormability
HardwareMechanical PropertiesDuctility
HardwareMechanical PropertiesModerate Strength
ConsumerCompactsAppearanceAppearance
CompactsCorrosion ResistanceCorrosion Resistance
CompactsForming CharacteristicsFormability
CompactsMachining CharacteristicsExcellent Machinability
CompactsMechanical PropertiesDuctility
Costume JewelryAppearanceAppearance
Costume JewelryCorrosion ResistanceCorrosion Resistance
Costume JewelryForming CharacteristicsFormability
Costume JewelryMechanical PropertiesDuctility
Costume JewelryMechanical PropertiesModerate Strength
Lipstick CasesAppearanceAppearance
Lipstick CasesCorrosion ResistanceCorrosion Resistance
Lipstick CasesForming CharacteristicsFormability
Lipstick CasesMechanical PropertiesDuctility
Lipstick CasesMechanical PropertiesModerate Strength
ElectricalElectrical ConnectorsConductivity (Electrical)Electrical Conductivity
Electrical ConnectorsCorrosion ResistanceCorrosion Resistance
Electrical ConnectorsForming CharacteristicsFormability
Electrical ConnectorsMechanical PropertiesModerate Strength
Flat Springs for Electrical Switch gearCorrosion ResistanceCorrosion Resistance
Flat Springs for Electrical Switch gearForming CharacteristicsFormability
Flat Springs for Electrical Switch gearMechanical PropertiesDuctility
Flat Springs for Electrical Switch gearMechanical PropertiesModerate Strength
Flat Springs for Electrical Switch gearThermal PropertiesResistance to Stress Relaxation
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsForming CharacteristicsFormability
Fuse ClipsMechanical PropertiesModerate Strength
Fuse ClipsThermal PropertiesResistance to Stress Relaxation
FastenersFastenersCorrosion ResistanceCorrosion Resistance
FastenersForming CharacteristicsFormability
FastenersMechanical PropertiesDuctility
FastenersMechanical PropertiesModerate Strength
FastenersThermal PropertiesResistance to Stress Relaxation
ScrewsCorrosion ResistanceCorrosion Resistance
ScrewsForming CharacteristicsFormability
ScrewsMechanical PropertiesDuctility
ScrewsMechanical PropertiesModerate Strength
IndustrialBearingsCorrosion ResistanceCorrosion Resistance
BearingsForming CharacteristicsFormability
BearingsFriction & Wear PropertiesWear Resistance
BearingsMechanical PropertiesDuctility
BearingsMechanical PropertiesModerate Strength
BearingsThermal PropertiesResistance to Stress Relaxation
BushingsCorrosion ResistanceCorrosion Resistance
BushingsForming CharacteristicsFormability
BushingsFriction & Wear PropertiesWear Resistance
BushingsMechanical PropertiesDuctility
BushingsMechanical PropertiesModerate Strength
BushingsThermal PropertiesResistance to Stress Relaxation
Plater Bar for JewelryAppearanceAppearance
Plater Bar for JewelryPlating CharacteristicsPlateable
Thrust WashersCorrosion ResistanceCorrosion Resistance
Thrust WashersForming CharacteristicsFormability
Thrust WashersFriction & Wear PropertiesWear Resistance
Thrust WashersMechanical PropertiesDuctility
Thrust WashersMechanical PropertiesModerate Strength
Thrust WashersThermal PropertiesResistance to Stress Relaxation
Applicable Specifications
Form System Standard Description
BarASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
PlateASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
SheetASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
StripASTMB591COPPER-ZINC-TIN ALLOY PLATE, SHEET, STRIP, AND ROLLED BAR
Corrosion Properties

No information available.