Find suppliers for this alloy
C46250
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P | Mg | |
|
(1) Includes Lanthanum 0.01-0.08 (2) Cu + Sum of Named Elements 99.5% min. |
|||||||
| Min (%) | 62.0 | .50 | .05 | .05 | |||
| Max (%) | 65.0 | .09 | 1.0 | 37.0 | .10 | .15 | .20 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Rod | Light Anneal | O50 |
65.3 Typ |
56.7 Typ |
20 Typ |
60 Typ |
| Melting Point - Liquidus°F | 1670 |
|---|---|
| Melting Point - Solidus°F | 1620 |
| Densitylb/cu in. at 68°F | 0.302 |
| Specific Gravity | 8.35 |
| Electrical Conductivity% IACS at 68°F | 26 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 138.6 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 12.4 |
| Modulus of Elasticity in Tensionksi | 6600 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties