Find suppliers for this alloyC48600
Chemical Composition
Element
Cu(1)PbSnZnAs
(1) Cu + Sum of Named Elements 99.6% min.
Min (%)59.01.00.300.02
Max (%)62.02.51.5Rem0.25
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Section Size
(in)
Rod & Wire1/2 HardH0250   Typ
25   Typ
10   Typ
60   Min
80   Max
1/2-1
H0240   Typ
15   Typ
35   Typ
35   Min
45   Max
>2
H0265   Typ
30   Typ
5   Typ
75   Min
80   Max
=<1/2
H0245   Typ
20   Typ
20   Typ
40   Min
75   Max
1-2
Soft AnnealO6040   Typ
15   Typ
25   Typ
40   Min
70   Max
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1645
Melting Point - Solidus°F1635
Densitylb/cu in. at 68°F0.304
Specific Gravity8.42
Electrical Conductivity% IACS at 68°F25
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)13
Modulus of Elasticity in Tensionksi14600
Fabrication Properties

No fabrication properties for this alloy

Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical Uses

No information available.

Applicable Specifications
Form Sub-Form System Standard Description
Forgings, Die (Hot Pressed)ASMESB283COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
ASTMB283/B283MCOPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
Rod, Bar & ShapesForgingsASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
Corrosion Properties

No information available.