| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | P | Bi | Cd | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
|||||||||
| Min (%) | 58.0 | 0.09 | 0.05 | 0.50 | |||||
| Max (%) | 62.0 | 0.25 | 0.50 | Rem | 0.30 | 0.12 | 1.3 | 0.001 | 0.10 |
| Form | Temper | Temper Code | YS-0.5% Ext (ksi) |
Elongation (%) |
Ultimate Tensile Strength in Shear (ksi) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Die Forging | As Hot Forged - Air Cooled | M10 | 22 Min |
25 Min |
52 Min |
| Melting Point - Liquidus°F | 1670 |
|---|---|
| Melting Point - Solidus°F | 1623 |
| Densitylb/cu in. at 68°F | 0.301 |
| Specific Gravity | 8.4 |
| Electrical Conductivity% IACS at 68°F | 21.7 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 45.5 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 7.33 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10.1 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15800 |
| Modulus of Rigidityksi | 5600 |
| Magnetic Permeability | 1.58 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Capacity for Being Cold Worked | Fair |
| Capacity for Being Hot Formed | Fair |
| Forgeability Rating | 70 |
| Machinability Rating | 90 |
Common Fabrication Processes
| Treatment | Minimum* | |||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 932 | |||
| Hot Working Temperature | 1210 | |||
| Stress Relief | 572 | |||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Automotive | Electrical & Electronic parts | ||
| Plumbing | Enviornmently Friendly Facuets and Plumbing Components |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| ASTM | B974/B974M | FREE-CUTTING BISMUTH BRASS ROD, BAR AND WIRE | |||
| ASTM | B967/B967M | COPPER-ZINC-TIN-BISMUTH ALLOY ROD, BAR AND WIRE | |||
| ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | |||
| Forgings, Die (Hot Pressed) | ASME | SB283 | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | ||
| ASTM | B283/B283M | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) |
Corrosion Properties