Find suppliers for this alloy
C49350
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Bi | Sb | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||||
| Min (%) | 61.0 | 1.5 | 0.04 | 0.50 | 0.02 | ||||
| Max (%) | 63.0 | 0.09 | 3.0 | Rem | 0.12 | 0.15 | 2.5 | 0.10 | 0.30 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 500 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Plumbing Fittings | As Hot Forged - Air Cooled | M10 |
49 Min 54 Typ 58 Max |
29 Min 33 Typ 36 Max |
20 Typ |
120 Typ |
| Melting Point - Liquidus°F | 1625 |
|---|---|
| Melting Point - Solidus°F | 1517 |
| Densitylb/cu in. at 68°F | 0.311 |
| Specific Gravity | 8.45 |
| Electrical Conductivity% IACS at 68°F | 19.8 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 48.7 |
| Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 10.8 |
| Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 11.2 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 14800 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Good |
| Capacity for Being Cold Worked | Poor |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 90 |
| Machinability Rating | 70 |
Common Fabrication Processes
Thermal Properties
Typical Uses
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Forgings, Die (Hot Pressed) | ASTM | B283/B283M | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | ||
| ASME | SB283 | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | |||
| Rod, Bar & Shapes | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | ||
| Rod, Bar & Wire | ASTM | B967/B967M | COPPER-ZINC-TIN-BISMUTH ALLOY ROD, BAR AND WIRE |
Corrosion Properties