Find suppliers for this alloy
C50100
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Fe | P | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||
| Min (%) | 0.50 | 0.01 | |||
| Max (%) | Rem | 0.05 | 0.8 | 0.05 | 0.05 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell 30T scale |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Tube | Annealed | O61 |
32.6 Min 40.6 Typ |
11 Typ |
40 Typ |
35 Typ |
| Melting Point - Liquidus°F | 1980 |
|---|---|
| Melting Point - Solidus°F | 1953 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.82 |
| Electrical Conductivity% IACS at 68°F | 55 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 131 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Telephone Cord Sets | Conductivity (Electrical) | Electrical Conductivity |
| Telephone Cord Sets | Mechanical Properties | Spring Properties | |
| Telephone Cord Sets | Pressure Tight | Pressure Tight | |
| Industrial | Pipe & Tube |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Wire | ASTM | B105 | HARD-DRAWN COPPER ALLOY WIRES FOR ELECTRICAL CONDUCTORS |
Corrosion Properties