Find suppliers for this alloyC50100
Chemical Composition
Element
Cu(1)PbSnFeP
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)0.500.01
Max (%)Rem0.050.80.050.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell 30T scale
TubeAnnealedO6132.6   Min
40.6   Typ
11   Typ
40   Typ
35   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1980
Melting Point - Solidus°F1953
Densitylb/cu in. at 68°F0.32
Specific Gravity8.82
Electrical Conductivity% IACS at 68°F55
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F131
Fabrication Properties
Technique Suitability
SolderingExcellent
Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
ElectricalTelephone Cord SetsConductivity (Electrical)Electrical Conductivity
Telephone Cord SetsMechanical PropertiesSpring Properties
Telephone Cord SetsPressure TightPressure Tight
IndustrialPipe & Tube
Applicable Specifications
Form System Standard Description
WireASTMB105HARD-DRAWN COPPER ALLOY WIRES FOR ELECTRICAL CONDUCTORS
Corrosion Properties

No information available.