Find suppliers for this alloy
C50580
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | Ni | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
|||||||
| Min (%) | 1.0 | 0.05 | 0.01 | 0.05 | |||
| Max (%) | Rem | 0.05 | 1.7 | 0.30 | 0.20 | 0.35 | 0.20 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Flat Products | 1/2 Hard | H02 |
65 Typ |
60 Typ |
12 Typ |
| 1/4 Hard | H01 |
58 Typ |
39 Typ |
24 Typ |
|
| Extra Hard | H06 |
80 Typ |
77 Typ |
6 Typ |
|
| Extra Spring | H10 |
89 Typ |
87 Typ |
2 Typ |
|
| Hard | H04 |
74 Typ |
72 Typ |
8 Typ |
|
| Nominal Grain Size 0.015 mm | OS015 |
53 Typ |
29 Typ |
50 Typ |
|
| Spring | H08 |
85 Typ |
83 Typ |
3 Typ |
|
| Melting Point - Liquidus°F | 1970 |
|---|---|
| Melting Point - Solidus°F | 1900 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.89 |
| Electrical Conductivity% IACS at 68°F | 41 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 130 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.9 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Good |
| Seam Weld | Fair |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 20 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 700 | 1350 | ||
Typical Uses
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Strip | ASTM | B888/B88M | COPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS |
Corrosion Properties