Find suppliers for this alloy
C50710
| Elements | ||||
|---|---|---|---|---|
| Cu(1) | Sn | P | Ni | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
||||
| Min (%) | 1.7 | 0.10 | ||
| Max (%) | Rem | 2.3 | 0.15 | 0.40 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm | Section Size (in) |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Strip | 1/2 Hard | H02 |
59.5 Min 74.0 Max |
10 Min |
125 Min 165 Max |
.10 |
| Annealed | O61 |
45.7 Min |
30 Min |
70 Min 115 Max |
.10 | |
| Extra Hard | H06 |
78.3 Min 92.1 Max |
2 Min |
175 Min 205 Max |
.10 | |
| Hard | H04 |
71.1 Min 85.6 Max |
5 Min |
150 Min 185 Max |
.10 | |
| Spring | H08 |
88.5 Min 102.3 Max |
185 Min |
.10 | ||
| Melting Point - Liquidus°F | 1949 |
|---|---|
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.88 |
| Electrical Conductivity% IACS at 68°F | 32 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 89.5 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.81 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.089 |
| Modulus of Elasticity in Tensionksi | 18100 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties