C50715
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1) | Pb | Sn(2) | Fe(3) | P(4) | |
|
(1) Cu + Sn + Fe + P 99.5% min (2) Cu + Sn + Fe + P 99.5% min (3) Cu + Sn + Fe + P 99.5% min (4) Cu + Sn + Fe + P 99.5% min |
|||||
| Min (%) | 1.7 | 0.05 | 0.025 | ||
| Max (%) | Rem | 0.02 | 2.3 | 0.15 | 0.04 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Flat Products | 1/2 Hard | H02 |
57 Min 73 Max |
42 Min 60 Max |
15 Min 25 Max |
| Extra Hard | H06 |
81 Min 95 Max |
74 Min 90 Max |
5 Min 10 Max |
|
| Extra Spring | H10 |
75 Min 84 Max |
73 Min 82 Max |
||
| Hard | H04 |
74 Min 87 Max |
64 Min 79 Max |
8 Min 16 Max |
|
| Spring | H08 |
86 Min 100 Max |
79 Min 94 Max |
3 Min 6 Max |
|
| Densitylb/cu in. at 68°F | 0.32 |
|---|---|
| Electrical Conductivity% IACS at 68°F | 48 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 120 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.9 |
| Modulus of Elasticity in Tensionksi | 17000 |
Fabrication Properties
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties