Find suppliers for this alloy
C51100
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
||||||
| Min (%) | 3.5 | 0.03 | ||||
| Max (%) | Rem | 0.05 | 4.9 | 0.30 | 0.10 | 0.35 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Torsion Modulus (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||||||
| Flat Products | 1/2 Hard | H02 |
103 Typ |
49 Typ |
54 Typ |
27 Typ |
70 Typ |
65 Typ |
0.04 | ||
| 1/2 Hard and Stress Relieved | HR02 |
63 Typ |
51 Typ |
26 Typ |
|||||||
| 1/4 Hard | H01 |
55 Typ |
43 Typ |
50 Typ |
36 Typ |
48 Typ |
45 Typ |
0.04 | |||
| 1/4 Hard | H01 |
55 Typ |
43 Typ |
36 Typ |
0.04 | ||||||
| 3/4 Hard | H03 |
74 Typ |
72 Typ |
11 Typ |
84 Typ |
72 Typ |
0.04 | ||||
| Extra Hard | H06 |
92 Typ |
89 Typ |
4 Typ |
91 Typ |
78 Typ |
0.04 | ||||
| Extra Spring | H10 |
103 Typ |
98 Typ |
80 Typ |
2 Typ |
95 Typ |
80 Typ |
0.04 | |||
| Hard | H04 |
80 Typ |
76 Typ |
74 Typ |
8 Typ |
86 Typ |
74 Typ |
41 Typ | 0.04 | ||
| Hard and Stress Relieved | HR04 |
80 Typ |
73 Typ |
15 Typ |
|||||||
| Nominal Grain Size 0.015 mm | OS015 |
51 Typ |
23 Typ |
46 Typ |
0.04 | ||||||
| Nominal Grain Size 0.015 mm | OS015 |
49 Typ |
23 Typ |
50 Typ |
76 Typ |
0.04 | |||||
| Nominal Grain Size 0.025 mm | OS025 |
50 Typ |
21 Typ |
46 Typ |
75 Typ |
0.04 | |||||
| Nominal Grain Size 0.035 mm | OS035 |
48 Typ |
19 Typ |
47 Typ |
73 Typ |
0.04 | |||||
| Nominal Grain Size 0.050 mm | OS050 |
46 Typ |
16 Typ |
48 Typ |
0.04 | ||||||
| Nominal Grain Size 0.050 mm | OS050 |
46 Typ |
16 Typ |
48 Typ |
70 Typ |
0.04 | |||||
| Spring | H08 |
103 Typ |
99 Typ |
80 Typ |
1 Typ |
93 Typ |
79 Typ |
0.04 | |||
| Spring and Stress Relieved | HR08 |
98 Typ |
88 Typ |
8 Typ |
|||||||
| Melting Point - Liquidus°F | 1945 |
|---|---|
| Melting Point - Solidus°F | 1785 |
| Densitylb/cu in. at 68°F | 0.32 |
| Specific Gravity | 8.86 |
| Electrical Conductivity% IACS at 68°F | 20 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 48.4 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Modulus of Rigidityksi | 6000 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Good |
| Seam Weld | Fair |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Poor |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Drawing
- Forming and Bending
- Roll Threading and Knurling
- Shearing
- Stamping
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 900 | 1250 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Architecture | Bridge Bearing Plates | Corrosion Resistance | Corrosion Resistance |
| Bridge Bearing Plates | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Bridge Bearing Plates | Forming Characteristics | Formability | |
| Bridge Bearing Plates | Mechanical Properties | Moderate to High Strength | |
| Electrical | Electronic Connectors | Conductivity (Electrical) | Electrical Conductivity |
| Electronic Connectors | Forming Characteristics | Excellent Formability | |
| Electronic Connectors | Mechanical Properties | Moderate Strength | |
| Electronic Connectors | Thermal Properties | Resistance to Stress Relaxation | |
| Fuse Clips | Conductivity (Electrical) | Electrical Conductivity | |
| Fuse Clips | Conductivity (Thermal) | High Thermal Conductivity | |
| Fuse Clips | Corrosion Resistance | Corrosion Resistance | |
| Fuse Clips | Mechanical Properties | Moderate to High Strength | |
| Fuse Clips | Solderability | Solderability | |
| Switch Parts | Conductivity (Electrical) | Electrical Conductivity | |
| Switch Parts | Conductivity (Thermal) | High Thermal Conductivity | |
| Switch Parts | Corrosion Resistance | Corrosion Resistance | |
| Switch Parts | Mechanical Properties | Moderate to High Strength | |
| Switch Parts | Solderability | Solderability | |
| Switch Parts | Thermal Properties | Resistance to Stress Relaxation | |
| Terminals | Conductivity (Electrical) | Electrical Conductivity | |
| Terminals | Conductivity (Thermal) | High Thermal Conductivity | |
| Terminals | Forming Characteristics | Formability | |
| Terminals | Mechanical Properties | Moderate to High Strength | |
| Terminals | Solderability | Solderability | |
| Terminals | Thermal Properties | Resistance to Stress Relaxation | |
| Fasteners | Fasteners | Corrosion Resistance | Corrosion Resistance |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Acids | |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Fasteners | Mechanical Properties | Moderate Strength | |
| Lock Washers | Corrosion Resistance | Corrosion Resistance | |
| Lock Washers | Forming Characteristics | Formability | |
| Lock Washers | Mechanical Properties | Moderate to High Strength | |
| Industrial | Beater Bar | Corrosion Resistance | Corrosion Resistance |
| Beater Bar | Corrosion Resistance | Corrosion Resistance to Acids | |
| Beater Bar | Forming Characteristics | Formability | |
| Beater Bar | Mechanical Properties | Fatigue Resistance | |
| Beater Bar | Mechanical Properties | Moderate to High Strength | |
| Beater Bar | Thermal Properties | Resistance to Stress Relaxation | |
| Bellows | Corrosion Resistance | Corrosion Resistance | |
| Bellows | Forming Characteristics | Formability | |
| Bellows | Mechanical Properties | Moderate to High Strength | |
| Chemical hardware | Corrosion Resistance | Corrosion Resistance | |
| Chemical hardware | Corrosion Resistance | Corrosion Resistance to Acids | |
| Chemical hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Chemical hardware | Forming Characteristics | Formability | |
| Chemical hardware | Mechanical Properties | Moderate to High Strength | |
| Clutch Disks | Corrosion Resistance | Corrosion Resistance | |
| Clutch Disks | Forming Characteristics | Formability | |
| Clutch Disks | Mechanical Properties | Fatigue Resistance | |
| Clutch Disks | Mechanical Properties | Moderate to High Strength | |
| Diaphragms | Corrosion Resistance | Corrosion Resistance | |
| Diaphragms | Corrosion Resistance | Corrosion Resistance to Acids | |
| Diaphragms | Forming Characteristics | Formability | |
| Diaphragms | Mechanical Properties | Fatigue Resistance | |
| Diaphragms | Mechanical Properties | Moderate to High Strength | |
| Perforated Sheets | Corrosion Resistance | Corrosion Resistance | |
| Perforated Sheets | Forming Characteristics | Formability | |
| Perforated Sheets | Mechanical Properties | Moderate Strength | |
| Sleeve Bushings | Corrosion Resistance | Corrosion Resistance | |
| Sleeve Bushings | Forming Characteristics | Formability | |
| Sleeve Bushings | Mechanical Properties | Ductility | |
| Sleeve Bushings | Mechanical Properties | Moderate to High Strength | |
| Springs | Forming Characteristics | Formability | |
| Springs | Mechanical Properties | Fatigue Resistance | |
| Springs | Mechanical Properties | High Strength | |
| Springs | Thermal Properties | Resistance to Stress Relaxation | |
| Textile machinery | Corrosion Resistance | Corrosion Resistance | |
| Textile machinery | Mechanical Properties | Moderate to High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Bearings & Busings | MILITARY | MIL-B-13501 | BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED | ||
| Plate | ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Bridge and Bearing | ASTM | B100 | ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES | ||
| Sheet | Bridge and Bearing | ASTM | B100 | ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES | |
| ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | |||
| Strip | ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | ||
| ASTM | B888/B88M | COPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS |
Corrosion Properties