Chemical Composition
Element
Cu(1)PbSnZnFeP
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)3.50.03
Max (%)Rem0.054.90.300.100.35
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Rockwell 30T scale
Torsion Modulus
(ksi)
Section Size
(in)
Flat Products1/2 HardH02103   Typ
63   Typ
94   Typ
49   Typ
54   Typ
27   Typ
7   Typ
70   Typ
65   Typ
0.04
1/2 Hard and Stress RelievedHR0263   Typ
51   Typ
26   Typ
1/4 HardH0155   Typ
43   Typ
50   Typ
36   Typ
48   Typ
45   Typ
0.04
H0155   Typ
43   Typ
36   Typ
0.04
3/4 HardH0374   Typ
72   Typ
11   Typ
84   Typ
72   Typ
0.04
Extra HardH0692   Typ
89   Typ
4   Typ
91   Typ
78   Typ
0.04
Extra SpringH10103   Typ
98   Typ
80   Typ
2   Typ
95   Typ
80   Typ
0.04
HardH0480   Typ
76   Typ
74   Typ
8   Typ
86   Typ
74   Typ
41   Typ
0.04
Hard and Stress RelievedHR0480   Typ
73   Typ
15   Typ
Nominal Grain Size 0.015 mmOS01551   Typ
23   Typ
46   Typ
0.04
OS01549   Typ
23   Typ
50   Typ
76   Typ
0.04
Nominal Grain Size 0.025 mmOS02550   Typ
21   Typ
46   Typ
75   Typ
0.04
Nominal Grain Size 0.035 mmOS03548   Typ
19   Typ
47   Typ
73   Typ
0.04
Nominal Grain Size 0.050 mmOS05046   Typ
16   Typ
48   Typ
0.04
OS05046   Typ
16   Typ
48   Typ
70   Typ
0.04
SpringH08103   Typ
99   Typ
80   Typ
1   Typ
93   Typ
79   Typ
0.04
Spring and Stress RelievedHR0898   Typ
88   Typ
8   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1945
Melting Point - Solidus°F1785
Densitylb/cu in. at 68°F0.32
Specific Gravity8.86
Electrical Conductivity% IACS at 68°F20
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F48.4
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.9
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingFair
Spot WeldGood
Seam WeldFair
Butt WeldExcellent
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedPoor
Machinability Rating20
Common Fabrication Processes
  • Blanking
  • Drawing
  • Forming and Bending
  • Roll Threading and Knurling
  • Shearing
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing9001250
Typical uses
Product Category Product Reason Category Reason
ArchitectureBridge Bearing PlatesCorrosion ResistanceCorrosion Resistance
Bridge Bearing PlatesCorrosion ResistanceCorrosion Resistance to Salt Water
Bridge Bearing PlatesForming CharacteristicsFormability
Bridge Bearing PlatesMechanical PropertiesModerate to High Strength
ElectricalElectronic ConnectorsConductivity (Electrical)Electrical Conductivity
Electronic ConnectorsForming CharacteristicsExcellent Formability
Electronic ConnectorsMechanical PropertiesModerate Strength
Electronic ConnectorsThermal PropertiesResistance to Stress Relaxation
Fuse ClipsConductivity (Electrical)Electrical Conductivity
Fuse ClipsConductivity (Thermal)High Thermal Conductivity
Fuse ClipsCorrosion ResistanceCorrosion Resistance
Fuse ClipsMechanical PropertiesModerate to High Strength
Fuse ClipsSolderabilitySolderability
Switch PartsConductivity (Electrical)Electrical Conductivity
Switch PartsConductivity (Thermal)High Thermal Conductivity
Switch PartsCorrosion ResistanceCorrosion Resistance
Switch PartsMechanical PropertiesModerate to High Strength
Switch PartsSolderabilitySolderability
Switch PartsThermal PropertiesResistance to Stress Relaxation
TerminalsConductivity (Electrical)Electrical Conductivity
TerminalsConductivity (Thermal)High Thermal Conductivity
TerminalsForming CharacteristicsFormability
TerminalsMechanical PropertiesModerate to High Strength
TerminalsSolderabilitySolderability
TerminalsThermal PropertiesResistance to Stress Relaxation
FastenersFastenersCorrosion ResistanceCorrosion Resistance
FastenersCorrosion ResistanceCorrosion Resistance to Acids
FastenersCorrosion ResistanceCorrosion Resistance to Salt Water
FastenersMechanical PropertiesModerate Strength
Lock WashersCorrosion ResistanceCorrosion Resistance
Lock WashersForming CharacteristicsFormability
Lock WashersMechanical PropertiesModerate to High Strength
IndustrialBeater BarCorrosion ResistanceCorrosion Resistance
Beater BarCorrosion ResistanceCorrosion Resistance to Acids
Beater BarForming CharacteristicsFormability
Beater BarMechanical PropertiesFatigue Resistance
Beater BarMechanical PropertiesModerate to High Strength
Beater BarThermal PropertiesResistance to Stress Relaxation
BellowsCorrosion ResistanceCorrosion Resistance
BellowsForming CharacteristicsFormability
BellowsMechanical PropertiesModerate to High Strength
Chemical hardwareCorrosion ResistanceCorrosion Resistance
Chemical hardwareCorrosion ResistanceCorrosion Resistance to Acids
Chemical hardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Chemical hardwareForming CharacteristicsFormability
Chemical hardwareMechanical PropertiesModerate to High Strength
Clutch DisksCorrosion ResistanceCorrosion Resistance
Clutch DisksForming CharacteristicsFormability
Clutch DisksMechanical PropertiesFatigue Resistance
Clutch DisksMechanical PropertiesModerate to High Strength
DiaphragmsCorrosion ResistanceCorrosion Resistance
DiaphragmsCorrosion ResistanceCorrosion Resistance to Acids
DiaphragmsForming CharacteristicsFormability
DiaphragmsMechanical PropertiesFatigue Resistance
DiaphragmsMechanical PropertiesModerate to High Strength
Perforated SheetsCorrosion ResistanceCorrosion Resistance
Perforated SheetsForming CharacteristicsFormability
Perforated SheetsMechanical PropertiesModerate Strength
Sleeve BushingsCorrosion ResistanceCorrosion Resistance
Sleeve BushingsForming CharacteristicsFormability
Sleeve BushingsMechanical PropertiesDuctility
Sleeve BushingsMechanical PropertiesModerate to High Strength
SpringsForming CharacteristicsFormability
SpringsMechanical PropertiesFatigue Resistance
SpringsMechanical PropertiesHigh Strength
SpringsThermal PropertiesResistance to Stress Relaxation
Textile machineryCorrosion ResistanceCorrosion Resistance
Textile machineryMechanical PropertiesModerate to High Strength
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
BarASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
Bearings & BusingsMILITARYMIL-B-13501BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED
PlateBridge and BearingASTMB100ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES
ASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
SheetBridge and BearingASTMB100ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES
ASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
StripASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
Electric Connector & Spring ContactASTMB888/B88MCOPPER ALLOY STRIP FOR USE IN MANUFACTURE OF ELECTRICAL CONNECTORS OR SPRING CONTACTS
Corrosion Properties

No information available.