Find suppliers for this alloyC51190
Chemical Composition
Element
Cu(1)PbSnFePCo
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)3.00.050.025
Max (%)Rem0.026.50.150.0450.15
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.2% Offset
Elongation
(%)
Vickers Hardness, 500 gm
Fatigue Strength**
(ksi)
Proportional Limit
(ksi)
Section Size
(in)
Flat Products1/2 HardH0281   Typ
78   Typ
16   Typ
185   Typ
77   Typ
Extra HardH06100   Typ
98   Typ
10   Typ
228   Typ
88   Typ
HardH0494   Typ
92   Typ
11   Typ
215   Typ
39   Typ
87   Typ
0.009
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1927
Melting Point - Solidus°F1742
Densitylb/cu in. at 68°F0.321
Specific Gravity8.9
Electrical Conductivity% IACS at 68°F22
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F53.2
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi11500
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingFair
Spot WeldGood
Seam WeldFair
Butt WeldExcellent
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedGood
Machinability Rating20
Fabrication Process Properties

No fabrication process properties for this alloy

    
Thermal Properties
Treatment Minimum* Maximum* Value*
* Temperature is measured in Fahrenheit.
Stress Relief523
Annealing842
Hot Treatment14721742
Typical Uses

No information available.

Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.