Find suppliers for this alloy
C52400
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | P | |
|
(1) Cu + Sum of Named Elements 99.5% min. |
||||||
| Min (%) | 9.0 | 0.03 | ||||
| Max (%) | Rem | 0.05 | 11.0 | 0.20 | 0.10 | 0.35 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Torsion Modulus (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||||
| Flat Products | 1/2 Hard | H02 |
83 Typ |
32 Typ |
92 Typ |
0.04 | ||
| Extra Hard | H06 |
115 Typ |
7 Typ |
100 Typ |
0.04 | |||
| Extra Spring | H10 |
128 Typ |
3 Typ |
103 Typ |
6 Typ | 0.04 | ||
| Hard | H04 |
100 Typ |
13 Typ |
97 Typ |
0.04 | |||
| Nominal Grain Size 0.035 mm | OS035 |
66 Typ |
28 Typ |
68 Typ |
55 Typ |
0.04 | ||
| Spring | H08 |
122 Typ |
4 Typ |
101 Typ |
0.04 | |||
| Flat Products & Wire | 1/2 Hard | H02 |
83 Typ |
32 Typ |
0.04 | |||
| 1/2 Hard | H02 |
118 Typ |
0.08 | |||||
| Hard | H04 |
147 Typ |
0.08 | |||||
| Hard | H04 |
100 Typ |
13 Typ |
0.04 | ||||
| Nominal Grain Size 0.035 mm | OS035 |
66 Typ |
70 Typ |
0.08 | ||||
| Nominal Grain Size 0.035 mm | OS035 |
66 Typ |
68 Typ |
0.04 | ||||
| Wire | 1/2 Hard | H02 |
118 Typ |
0.08 | ||||
| 1/4 Hard | H01 |
93 Typ |
0.08 | |||||
| Hard | H04 |
147 Typ |
0.08 | |||||
| Nominal Grain Size 0.035 mm | OS035 |
66 Typ |
70 Typ |
0.08 | ||||
| Melting Point - Liquidus°F | 1830 |
|---|---|
| Melting Point - Solidus°F | 1550 |
| Densitylb/cu in. at 68°F | 0.317 |
| Specific Gravity | 8.78 |
| Electrical Conductivity% IACS at 68°F | 11 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 29 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Modulus of Rigidityksi | 6000 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Good |
| Seam Weld | Fair |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Poor |
| Machinability Rating | 20 |
Common Fabrication Processes
- Bending
- Blanking
- Forming
- Shearing
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 900 | 1250 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Expansion Plates for Bridges | Corrosion Resistance | Corrosion Resistance |
| Expansion Plates for Bridges | Friction & Wear Properties | Wear Resistance | |
| Expansion Plates for Bridges | Mechanical Properties | High Strength | |
| Fittings | Corrosion Resistance | Corrosion Resistance | |
| Fittings | Mechanical Properties | High Strength | |
| Heavy Bars and Plates | Corrosion Resistance | Corrosion Resistance | |
| Heavy Bars and Plates | Forming Characteristics | Formability | |
| Heavy Bars and Plates | Friction & Wear Properties | Wear Resistance | |
| Heavy Bars and Plates | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | ||
| ASTM | B139/B139M | PHOSPHOR BRONZE ROD, BAR AND SHAPES | |||
| Plate | ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Rod | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Welding | AWS | A5.13 | SURFACE WELDING RODS AND ELECTRODES | ||
| ASTM | B139/B139M | PHOSPHOR BRONZE ROD, BAR AND SHAPES | |||
| Shapes | ASTM | B139/B139M | PHOSPHOR BRONZE ROD, BAR AND SHAPES | ||
| Sheet | ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | ||
| Strip | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| ASTM | B103/B103M | PHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR | |||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Wire | ASTM | B159/B159M | PHOSPHOR BRONZE WIRE |
Corrosion Properties