Find suppliers for this alloyC52400
Chemical Composition
Element
Cu(1)PbSnZnFeP
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)9.00.03
Max (%)Rem0.0511.00.200.100.35
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Torsion Modulus
(ksi)
Section Size
(in)
Flat Products1/2 HardH0283   Typ
32   Typ
92   Typ
0.04
Extra HardH06115   Typ
7   Typ
100   Typ
0.04
Extra SpringH10128   Typ
3   Typ
103   Typ
6   Typ
0.04
HardH04100   Typ
13   Typ
97   Typ
0.04
Nominal Grain Size 0.035 mmOS03566   Typ
28   Typ
68   Typ
55   Typ
0.04
SpringH08122   Typ
4   Typ
101   Typ
0.04
Flat Products & Wire1/2 HardH0283   Typ
32   Typ
0.04
H02118   Typ
0.08
HardH04147   Typ
0.08
H04100   Typ
13   Typ
0.04
Nominal Grain Size 0.035 mmOS03566   Typ
70   Typ
0.08
OS03566   Typ
68   Typ
0.04
Wire1/2 HardH02118   Typ
0.08
1/4 HardH0193   Typ
0.08
HardH04147   Typ
0.08
Nominal Grain Size 0.035 mmOS03566   Typ
70   Typ
0.08
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1830
Melting Point - Solidus°F1550
Densitylb/cu in. at 68°F0.317
Specific Gravity8.78
Electrical Conductivity% IACS at 68°F11
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F29
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)10.2
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingFair
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingFair
Spot WeldGood
Seam WeldFair
Butt WeldExcellent
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedPoor
Machinability Rating20
Common Fabrication Processes
  • Bending
  • Blanking
  • Forming
  • Shearing
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing9001250
Typical uses
Product Category Product Reason Category Reason
IndustrialExpansion Plates for BridgesCorrosion ResistanceCorrosion Resistance
Expansion Plates for BridgesFriction & Wear PropertiesWear Resistance
Expansion Plates for BridgesMechanical PropertiesHigh Strength
FittingsCorrosion ResistanceCorrosion Resistance
FittingsMechanical PropertiesHigh Strength
Heavy Bars and PlatesCorrosion ResistanceCorrosion Resistance
Heavy Bars and PlatesForming CharacteristicsFormability
Heavy Bars and PlatesFriction & Wear PropertiesWear Resistance
Heavy Bars and PlatesMechanical PropertiesHigh Strength
Applicable Specifications
Form Application System Standard Description
BarASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
ASTMB139/B139MPHOSPHOR BRONZE ROD, BAR AND SHAPES
PlateASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
RodASTMB139/B139MPHOSPHOR BRONZE ROD, BAR AND SHAPES
WeldingAWSA5.13SURFACE WELDING RODS AND ELECTRODES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ShapesASTMB139/B139MPHOSPHOR BRONZE ROD, BAR AND SHAPES
SheetASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
StripASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
WireASTMB159/B159MPHOSPHOR BRONZE WIRE
Corrosion Properties

No information available.