Find suppliers for this alloyC54400
Chemical Composition
Element
Cu(1)PbSnZnFeP
(1) Cu + Sum of Named Elements 99.5% min.
Min (%)3.03.51.50.01
Max (%)Rem4.04.54.50.100.50
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Rockwell F scale
Torsion Modulus
(ksi)
Section Size
(in)
Cold Work
(%)
Flat Products1/2 HardH0258   Typ
40   Typ
24   Typ
68   Typ
0.04
HardH0460   Typ
45   Typ
20   Typ
0.315
Nominal Grain Size 0.035 mmOS03544   Typ
19   Typ
50   Typ
65   Typ
0.04
SpringH0898   Typ
80   Typ
3   Typ
0.04
RodHardH0468   Typ
57   Typ
20   Typ
80   Typ
5.7   Typ
125
H0475   Typ
63   Typ
15   Typ
83   Typ
0.535
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1830
Melting Point - Solidus°F1700
Densitylb/cu in. at 68°F0.32
Specific Gravity8.89
Electrical Conductivity% IACS at 68°F19
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F50
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.6
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi15000
Modulus of Rigidityksi5600
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingNot Recommended
Coated Metal Arc WeldingNot Recommended
Spot WeldNot Recommended
Seam WeldNot Recommended
Butt WeldFair
Capacity for Being Cold WorkedGood
Machinability Rating80
Common Fabrication Processes
  • Blanking
  • Drawing
  • Forming and Bending
  • Machining
  • Shearing
  • Stamping
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing9001250
Typical uses
Product Category Product Reason Category Reason
ElectricalElectrical ConnectorsCorrosion ResistanceStress Corrosion Cracking Resistance
Electrical ConnectorsMachining CharacteristicsMachinability
Electrical ConnectorsMechanical PropertiesHigh Endurance Limit
Electrical ConnectorsMechanical PropertiesHigh Strength
IndustrialBearingsCorrosion ResistanceCorrosion Resistance
BearingsFriction & Wear PropertiesWear Resistance
BearingsMachining PropertiesMachinability, Good
BearingsMechanical PropertiesModerate Strength
BushingsCorrosion ResistanceCorrosion Resistance
BushingsFriction & Wear PropertiesWear Resistance
BushingsMachining PropertiesMachinability, Good
BushingsMechanical PropertiesModerate Strength
GearsCorrosion ResistanceCorrosion Resistance
GearsFriction & Wear PropertiesWear Resistance
GearsMachining PropertiesMachinability, Good
GearsMechanical PropertiesModerate Strength
PinionsCorrosion ResistanceCorrosion Resistance
PinionsFriction & Wear PropertiesWear Resistance
PinionsMachining PropertiesMachinability, Good
PinionsMechanical PropertiesFatigue Resistance
PinionsMechanical PropertiesModerate Strength
Screw Machine ProductsCorrosion ResistanceCorrosion Resistance
Screw Machine ProductsMachining CharacteristicsMachinability
Screw Machine ProductsMechanical PropertiesModerate Strength
ShaftsCorrosion ResistanceCorrosion Resistance
ShaftsFriction & Wear PropertiesWear Resistance
ShaftsMachining PropertiesMachinability, Good
ShaftsMechanical PropertiesModerate Strength
Sleeve BearingsCorrosion ResistanceCorrosion Resistance
Sleeve BearingsFriction & Wear PropertiesWear Resistance
Sleeve BearingsMechanical PropertiesModerate Strength
Thrust BearingsCorrosion ResistanceCorrosion Resistance
Thrust BearingsFriction & Wear PropertiesWear Resistance
Thrust BearingsMechanical PropertiesModerate Strength
Thrust WashersCorrosion ResistanceCorrosion Resistance
Thrust WashersFriction & Wear PropertiesWear Resistance
Thrust WashersMachining PropertiesMachinability, Good
Thrust WashersMechanical PropertiesModerate Strength
Valve PartsCorrosion ResistanceCorrosion Resistance
Valve PartsFriction & Wear PropertiesWear Resistance
Valve PartsMachining PropertiesMachinability, Good
Valve PartsMechanical PropertiesModerate Strength
Applicable Specifications
Form Temper System Standard Description
BarASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
ASTMB139/B139MPHOSPHOR BRONZE ROD, BAR AND SHAPES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Bearings & BusingsMILITARYMIL-B-13501BEARINGS AND BUSHINGS, BRASS AND BRONZE MACHINED OR FORMED
PlateASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
RodASTMB139/B139MPHOSPHOR BRONZE ROD, BAR AND SHAPES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ShapesASTMB139/B139MPHOSPHOR BRONZE ROD, BAR AND SHAPES
SheetASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Strip1/2 HardAMS4520BRONZE STRIP, COLD ROLLED, HALF HARD
ASTMB103/B103MPHOSPHOR BRONZE PLATE, SHEET, STRIP AND ROLLED BAR
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.