Find suppliers for this alloy
C60800
| Elements | |||||
|---|---|---|---|---|---|
| Cu(1,2) | Pb | Fe | Al | As | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. |
|||||
| Min (%) | 5.0 | 0.02 | |||
| Max (%) | Rem | 0.10 | 0.10 | 6.5 | 0.35 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell F scale | Torsion Modulus (ksi) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| Tube | Nominal Grain Size 0.025 mm | OS025 |
60 Typ |
27 Typ |
55 Typ |
77 Typ |
6.7 Typ |
| Melting Point - Liquidus°F | 1945 |
|---|---|
| Melting Point - Solidus°F | 1920 |
| Densitylb/cu in. at 68°F | 0.295 |
| Specific Gravity | 8.17 |
| Electrical Conductivity% IACS at 68°F | 17 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 46 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17500 |
| Modulus of Rigidityksi | 6600 |
| Technique | Suitability |
|---|---|
| Soldering | Not Recommended |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Fair |
| Machinability Rating | 20 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1000 | 1200 | ||
| Hot Working Temperature | 1450 | 1600 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Builders Hardware | Hardware | Appearance | Appearance |
| Hardware | Corrosion Resistance | Corrosion Resistance | |
| Hardware | Mechanical Properties | Moderate Strength | |
| Fasteners | Fasteners | Corrosion Resistance | Corrosion Resistance |
| Fasteners | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Fasteners | Mechanical Properties | Moderate Strength | |
| Industrial | Condenser Tubes | Corrosion Resistance | Corrosion Resistance |
| Condenser Tubes | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Condenser Tubes | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Condenser Tubes | Forming Characteristics | Formability | |
| Condenser Tubes | Mechanical Properties | Moderate Strength | |
| Condenser Tubes | Mechanical Properties | Retains Strength at High Temperatures | |
| Distiller Tubes | Corrosion Resistance | Corrosion Resistance | |
| Distiller Tubes | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Distiller Tubes | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Distiller Tubes | Forming Characteristics | Formability | |
| Distiller Tubes | Mechanical Properties | Moderate Strength | |
| Distiller Tubes | Mechanical Properties | Retains Strength at High Temperatures | |
| Evaporator Tubing | Corrosion Resistance | Corrosion Resistance | |
| Evaporator Tubing | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Evaporator Tubing | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Evaporator Tubing | Forming Characteristics | Formability | |
| Evaporator Tubing | Mechanical Properties | Retains Strength at High Temperatures | |
| Ferrules | Corrosion Resistance | Corrosion Resistance | |
| Ferrules | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Ferrules | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Ferrules | Forming Characteristics | Formability | |
| Ferrules | Mechanical Properties | Moderate Strength | |
| Ferrules | Mechanical Properties | Retains Strength at High Temperatures | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Heat Exchanger Tubes | Forming Characteristics | Formability | |
| Heat Exchanger Tubes | Mechanical Properties | Moderate Strength | |
| Heat Exchanger Tubes | Mechanical Properties | Retains Strength at High Temperatures | |
| Seamless Tubing | Corrosion Resistance | Corrosion Resistance | |
| Seamless Tubing | Forming Characteristics | Formability | |
| Seamless Tubing | Mechanical Properties | Moderate Strength | |
| Structural Components | Corrosion Resistance | Corrosion Resistance | |
| Structural Components | Mechanical Properties | Moderate Strength | |
| Tanks, Corrosion Resistant | Corrosion Resistance | Corrosion Resistance | |
| Vessels, Corrosion Resistant | Corrosion Resistance | Corrosion Resistance | |
| Vessels, Corrosion Resistant | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Vessels, Corrosion Resistant | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Vessels, Corrosion Resistant | Mechanical Properties | Moderate Strength | |
| Marine | Protective Sheathing | Corrosion Resistance | Corrosion Resistance |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Protective Sheathing | Mechanical Properties | Moderate Strength | |
| Ordnance | Blending Chambers | Corrosion Resistance | Corrosion Resistance |
| Blending Chambers | Mechanical Properties | Moderate Strength | |
| Blending Chambers | Non-Sparking | Non-Sparking | |
| Mixing Troughs | Corrosion Resistance | Corrosion Resistance | |
| Mixing Troughs | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Mixing Troughs | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Mixing Troughs | Mechanical Properties | Moderate Strength | |
| Mixing Troughs | Non-Sparking | Non-Sparking |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Seamless Condenser Tube & Ferrule Stock | Condenser Tube | ASTM | B111/B111M | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK | |
| Condenser Tube | ASME | SB111 | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK | ||
| Seamless Heat Exchanger Tube with Integral Fins | ASTM | B359/B359M | COPPER AND COPPER-ALLOY SEAMLESS CONDENSER AND HEAT EXCHANGER TUBES WITH INTEGRAL FINS | ||
| ASME | SB359 | COPPER & COPPER ALLOY SEAMLESS CONDENSER & HEAT EXCHANGER TUBES WITH INTEGRAL FINS | |||
| Tubes, Seamless Condenser & Heat Exchanger, U-Bend | ASME | SB395 | U-BEND SEAMLESS COPPER & COPPER ALLOY HEAT EXCHANGER & CONDENSER TUBE | ||
| ASTM | B395/B395M | U-BEND SEAMLESS COPPER AND COPPER ALLOY HEAT EXCHANGER AND CONDENSER TUBES |
Corrosion Properties