C61300
| Elements | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn(3) | Fe | P | Ni(4) | Al | Mn | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.8% min. (3) When the product is for subsequent welding applications and is so specified by the purchaser, Cr, Cd, Zr, and Zn shall each be 0.05%max. (4) Ni value includes Co. |
||||||||||
| Min (%) | 0.20 | 2.0 | 6.0 | |||||||
| Max (%) | Rem | 0.01 | 0.50 | 0.10 | 3.0 | 0.015 | 0.15 | 7.5 | 0.20 | 0.10 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
YS-0.5% Ext (ksi) |
YS-0.05% Offset |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Izod (ft-lbs) |
Fatigue Strength** (ksi) |
Reduction of Area (%) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||||
| Flat Products | As Hot Rolled | M20 |
80 Typ |
40 Typ |
40 Typ |
82 Typ |
52 Typ |
28 Typ | >0.5 - 2 | |||||||
| As Hot Rolled | M20 |
72 Min for Standard |
30 Min for Standard |
32 Min for Standard |
35 Min for Standard |
>2.0 - 5 | ||||||||||
| As Hot Rolled | M20 |
75 Min for Standard |
34 Min for Standard |
35 Min for Standard |
81 Typ |
50 Typ |
=<0.5 | |||||||||
| Rod | Drawn and Stress Relieved | HR50 |
80 Min |
30 Min |
=<0.5 | |||||||||||
| Hard | H04 |
82 Typ |
55 Typ |
35 Typ |
90 Typ |
45 Typ |
1 | 25 | ||||||||
| Hard | H04 |
80 Typ |
48 Typ |
35 Typ |
88 Typ |
40 Typ |
6.4 Typ | 26 Typ | 2.4 Typ |
2 | 25 | |||||
| Hard | H04 |
85 Typ |
58 Typ |
35 Typ |
91 Typ |
48 Typ |
0.5 | 25 | ||||||||
| Rod, Bar & Shapes | Extruded and Drawn | H50 |
75 Min for Standard |
30 Min for Standard |
51 Typ | >1 to 2 | ||||||||||
| Tube | As Hot Extruded | M30 |
65 Min for Standard |
30 Min for Standard |
||||||||||||
| Melting Point - Liquidus°F | 1915 |
|---|---|
| Melting Point - Solidus°F | 1905 |
| Densitylb/cu in. at 68°F | 0.287 |
| Specific Gravity | 7.95 |
| Electrical Conductivity% IACS at 68°F | 12 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 32 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Not Recommended |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
| Forgeability Rating | 50 |
| Machinability Rating | 30 |
Common Fabrication Processes
- Blanking
- Cold Heading
- Drawing
- Forming and Bending
- Roll Threading
- Welding
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1125 | 1600 | ||
| Hot Working Temperature | 1450 | 1700 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Building | Wire Screening | Corrosion Resistance | Corrosion Resistance |
| Wire Screening | Forming Characteristics | Formability | |
| Wire Screening | Mechanical Properties | High Strength | |
| Fasteners | Bolts | Corrosion Resistance | Corrosion Resistance |
| Bolts | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Bolts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Bolts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Bolts | Forming Characteristics | Formability | |
| Bolts | Mechanical Properties | High Strength | |
| Fasteners | Corrosion Resistance | Corrosion Resistance | |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Acids | |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Fasteners | Mechanical Properties | High Strength | |
| Nuts | Corrosion Resistance | Corrosion Resistance | |
| Nuts | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Nuts | Forming Characteristics | Formability | |
| Nuts | Mechanical Properties | High Strength | |
| Industrial | Columns | Corrosion Resistance | Corrosion Resistance |
| Columns | Mechanical Properties | High Strength | |
| Condenser Tube | Corrosion Resistance | Corrosion Resistance | |
| Condenser Tube | Corrosion Resistance | Corrosion Resistance to Acids | |
| Condenser Tube | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Acids | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Corrosion Resistant Vessels | Mechanical Properties | High Strength | |
| Desalination Equipment | Corrosion Resistance | Corrosion Resistance | |
| Desalination Equipment | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Desalination Equipment | Mechanical Properties | High Strength | |
| Gaskets | Corrosion Resistance | Corrosion Resistance | |
| Gaskets | Corrosion Resistance | Corrosion Resistance to Acids | |
| Gaskets | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Gaskets | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Gaskets | Mechanical Properties | Strength | |
| Gaskets | Pressure Tight | Pressure Tight | |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Heat Exchanger Tube | Forming Characteristics | Formability | |
| Heat Exchanger Tube | Mechanical Properties | High Strength | |
| Heat Exchanger Tube | Welding Characteristics | Weldability | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Machine Parts | Forming Characteristics | Formability | |
| Machine Parts | Friction & Wear Properties | Wear Resistance | |
| Machine Parts | Mechanical Properties | High Strength | |
| Mining Shovels | Friction & Wear Properties | Wear Resistance | |
| Mining Shovels | Mechanical Properties | High Strength | |
| Mining Shovels | Non-Sparking | Non-Sparking | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance to Acids | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance to Non-Oxidizing Mineral Acids | |
| Piping Systems, Acid Resistant | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Piping Systems, Acid Resistant | Forming Characteristics | Formability | |
| Piping Systems, Acid Resistant | Mechanical Properties | High Strength | |
| Sea Water Piping | Corrosion Resistance | Corrosion Resistance | |
| Sea Water Piping | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Sea Water Piping | Mechanical Properties | High Strength | |
| Sea Water Piping | Welding Characteristics | Weldability | |
| Seamless Tubing and Pipe | Corrosion Resistance | Corrosion Resistance | |
| Seamless Tubing and Pipe | Forming Characteristics | Formability | |
| Seamless Tubing and Pipe | Mechanical Properties | High Strength | |
| Seamless Tubing and Pipe | Welding Characteristics | Weldability | |
| Tanks | Corrosion Resistance | Corrosion Resistance | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Tanks | Mechanical Properties | High Modulus of Elasticity | |
| Tanks | Welding Characteristics | Weldability | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Acids | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Tie Rods | Mechanical Properties | High Strength | |
| Tube Sheets | Corrosion Resistance | Corrosion Resistance | |
| Tube Sheets | Forming Characteristics | Formability | |
| Tube Sheets | Mechanical Properties | High Strength | |
| Water Boxes | Corrosion Resistance | Corrosion Resistance | |
| Water Boxes | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Water Boxes | Mechanical Properties | High Strength | |
| Marine | Marine Hardware | Corrosion Resistance | Corrosion Resistance |
| Marine Hardware | Corrosion Resistance | Stress Corrosion Cracking Resistance | |
| Marine Hardware | Mechanical Properties | High Strength | |
| Marine Hardware | Welding Characteristics | Weldable with C61000 | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Protective Sheathing | Mechanical Properties | High Strength | |
| Ordnance | Blending Chambers | Forming Characteristics | Formability |
| Blending Chambers | Mechanical Properties | High Strength | |
| Blending Chambers | Non-Sparking | Non-Sparking | |
| Mixing Troughs | Corrosion Resistance | Corrosion Resistance | |
| Mixing Troughs | Forming Characteristics | Formability | |
| Mixing Troughs | Mechanical Properties | High Strength | |
| Mixing Troughs | Non-Sparking | Non-Sparking | |
| Mixing Troughs | Welding Characteristics | Weldability | |
| Other | Ball Valve Seats | Corrosion Resistance | Corrosion Resistance |
| Ball Valve Seats | Corrosion Resistance | Corrosion Resistance to Acids | |
| Ball Valve Seats | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Ball Valve Seats | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | ||
| ASTM | B150/B150M | ALUMINUM BRONZE ROD, BAR AND SHAPES | |||
| ASTM | B169/B169M | ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND ROLLED BAR | |||
| Pipe | ASTM | B608 | WELDED COPPER ALLOY PIPE | ||
| Plate | FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | ||
| ASTM | B432 | COPPER AND COPPER ALLOY CLAD STEEL PLATE | |||
| ASTM | B169/B169M | ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND ROLLED BAR | |||
| Plate & Sheet | for Pressure Vessels, Condensers & Heat Exchangers | ASTM | B171/B171M | COPPER ALLOY CONDENSER TUBE PLATES | |
| for Pressure Vessels, Condensers & Heat Exchangers | ASME | SB171 | COPPER ALLOY CONDENSER TUBE PLATES | ||
| Rod | ASTM | B150/B150M | ALUMINUM BRONZE ROD, BAR AND SHAPES | ||
| Rod, Bar & Shapes | Aluminum Bronze | ASME | SB150 | ALUMINUM BRONZE ROD, BAR, AND SHAPES | |
| Rod, Tubing & Shapes | Aluminum Bronze | ASTM | B150/B150M | ALUMINUM BRONZE ROD, BAR AND SHAPES | |
| Seamless Condenser Tube & Ferrule Stock | ASME | SB111 | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK | ||
| ASTM | B100 | ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES | |||
| Seamless Pipe and Tube | ASTM | B315 | SEAMLESS COPPER ALLOY PIPE AND TUBE | ||
| ASME | SB315 | COPPER-SILICON ALLOY SEAMLESS PIPE AND TUBE | |||
| Sheet | ASTM | B169/B169M | ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | |||
| Sheet, Strip & Rolled Bar | Aluminum Bronze | ASME | SB169 | ALUMINUM BRONZE PLATE, SHEET, STRIP, AND ROLLED BAR | |
| Strip | ASTM | B169/B169M | ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | |||
| Tube | ASTM | B111/B111M | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK |
Corrosion Properties