Find suppliers for this alloy
C61400
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | P | Al | Mn | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
|||||||
| Min (%) | 1.5 | 6.0 | |||||
| Max (%) | Rem | 0.01 | 0.20 | 3.5 | 0.015 | 8.0 | 1.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Izod (ft-lbs) |
Fatigue Strength** (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
| Flat Products | Hard | H04 |
89 Typ |
60 Typ |
32 Typ |
87 Typ |
0.125 | |||||
| Hard | H04 |
85 Typ |
58 Typ |
35 Typ |
86 Typ |
0.312 | ||||||
| Hard | H04 |
78 Typ |
45 Typ |
40 Typ |
84 Typ |
1 | ||||||
| Hard | H04 |
80 Typ |
54 Typ |
38 Typ |
85 Typ |
48 Typ |
0.5 | |||||
| Soft Anneal | O60 |
80 Typ |
40 Typ |
40 Typ |
42 Typ |
0.315 | ||||||
| Soft Anneal | O60 |
80 Typ |
40 Typ |
40 Typ |
83 Typ |
42 Typ |
26 Typ | 0.312 | ||||
| Soft Anneal | O60 |
82 Typ |
45 Typ |
40 Typ |
84 Typ |
45 Typ |
30 Typ | 0.125 | ||||
| Soft Anneal | O60 |
82 Typ |
45 Typ |
40 Typ |
45 Typ |
0.118 | ||||||
| Soft Anneal | O60 |
76 Typ |
33 Typ |
45 Typ |
81 Typ |
28 Typ | 40 Typ |
1 | ||||
| Soft Anneal | O60 |
78 Typ |
35 Typ |
42 Typ |
40 Typ |
0.59 | ||||||
| Soft Anneal | O60 |
78 Typ |
35 Typ |
42 Typ |
82 Typ |
40 Typ |
25 Typ | 0.5 | ||||
| Rod | Drawn and Stress Relieved | HR50 |
75 Min for Standard |
30 Min for Standard |
1 | |||||||
| Drawn and Stress Relieved | HR50 |
80 Min for Standard |
30 Min for Standard |
0.5 | ||||||||
| Drawn and Stress Relieved | HR50 |
70 Min for Standard |
30 Min for Standard |
2 | ||||||||
| Hard | H04 |
85 Typ |
45 Typ |
35 Typ |
91 Typ |
48 Typ |
0.5 | |||||
| Hard | H04 |
82 Typ |
40 Typ |
35 Typ |
90 Typ |
45 Typ |
1 | |||||
| Hard | H04 |
80 Typ |
35 Typ |
35 Typ |
88 Typ |
40 Typ |
6.1 Typ | 26 Typ | 2 | |||
| Melting Point - Liquidus°F | 1915 |
|---|---|
| Melting Point - Solidus°F | 1905 |
| Densitylb/cu in. at 68°F | 0.285 |
| Specific Gravity | 7.89 |
| Electrical Conductivity% IACS at 68°F | 14 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 39 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Not Recommended |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Drawing
- Forming and Bending
- Heading and Roll Threading
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1125 | 1650 | ||
| Hot Working Temperature | 1450 | 1700 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Fasteners | Bolts | Corrosion Resistance | Corrosion Resistance |
| Bolts | Corrosion Resistance | Corrosion Resistance to Acids | |
| Bolts | Mechanical Properties | High Strength | |
| Nuts | Corrosion Resistance | Corrosion Resistance | |
| Nuts | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Nuts | Mechanical Properties | High Strength | |
| Stringers | Corrosion Resistance | Corrosion Resistance | |
| Stringers | Mechanical Properties | High Strength | |
| Threaded Members | Corrosion Resistance | Corrosion Resistance | |
| Threaded Members | Corrosion Resistance | Corrosion Resistance to Acids | |
| Threaded Members | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Threaded Members | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Threaded Members | Mechanical Properties | High Strength | |
| Industrial | Chutes for Abrasive Grains | Corrosion Resistance | Corrosion Resistance |
| Chutes for Abrasive Grains | Friction & Wear Properties | Wear Resistance | |
| Chutes for Abrasive Grains | Mechanical Properties | High Strength | |
| Condenser Head Plates | Corrosion Resistance | Corrosion Resistance | |
| Condenser Head Plates | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Condenser Head Plates | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Condenser Head Plates | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Condenser Head Plates | Mechanical Properties | High Strength | |
| Condenser Tube and Piping Systems | Corrosion Resistance | Corrosion Resistance | |
| Condenser Tube and Piping Systems | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Condenser Tube and Piping Systems | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Condenser Tube and Piping Systems | Mechanical Properties | High Strength | |
| Condenser Tube and Piping Systems | Welding Characteristics | Weldability | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Acids | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Non-Oxidizing Mineral Acids | |
| Corrosion Resistant Vessels | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Corrosion Resistant Vessels | Mechanical Properties | High Strength | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubes | Forming Characteristics | Formability | |
| Heat Exchanger Tubes | Mechanical Properties | High Strength | |
| Heat Exchanger Tubes | Welding Characteristics | Weldability | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Machine Parts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Machine Parts | Mechanical Properties | High Strength | |
| Mining Shovels | Corrosion Resistance | Corrosion Resistance | |
| Mining Shovels | Friction & Wear Properties | Wear Resistance | |
| Mining Shovels | Mechanical Properties | High Strength | |
| Mining Shovels | Non-Sparking | Non-Sparking | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance to Acids | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance to Non-Oxidizing Mineral Acids | |
| Piping Systems | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Piping Systems | Mechanical Properties | High Strength | |
| Sea Water Piping | Corrosion Resistance | Corrosion Resistance | |
| Sea Water Piping | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Sea Water Piping | Mechanical Properties | High Strength | |
| Sea Water Piping | Welding Characteristics | Weldability | |
| Seamless Tubing and Pipe | Corrosion Resistance | Corrosion Resistance | |
| Seamless Tubing and Pipe | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Seamless Tubing and Pipe | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Seamless Tubing and Pipe | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Seamless Tubing and Pipe | Forming Characteristics | Formability | |
| Seamless Tubing and Pipe | Mechanical Properties | High Strength | |
| Seamless Tubing and Pipe | Welding Characteristics | Weldability | |
| Structural Components | Corrosion Resistance | Corrosion Resistance | |
| Structural Components | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Structural Components | Mechanical Properties | High Strength | |
| Tanks | Corrosion Resistance | Corrosion Resistance | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Tanks | Mechanical Properties | High Strength | |
| Tanks | Welding Characteristics | Weldability | |
| Tube Sheets | Corrosion Resistance | Corrosion Resistance | |
| Tube Sheets | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Tube Sheets | Mechanical Properties | High Strength | |
| Tube Sheets | Welding Characteristics | Weldability | |
| Welded Pipe | Corrosion Resistance | Corrosion Resistance | |
| Welded Pipe | Mechanical Properties | High Strength | |
| Welded Pipe | Welding Characteristics | Weldability | |
| Marine | Fasteners | Corrosion Resistance | Corrosion Resistance |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Acids | |
| Fasteners | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Fasteners | Mechanical Properties | High Strength | |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance | |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Marine Hardware | Corrosion Resistance | Stress Corrosion Cracking Resistance | |
| Marine Hardware | Mechanical Properties | Moderate to High Strength | |
| Pressure Vessels | Corrosion Resistance | Corrosion Resistance | |
| Pressure Vessels | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Pressure Vessels | Corrosion Resistance | Stress Corrosion Cracking Resistance | |
| Pressure Vessels | Mechanical Properties | Moderate to High Strength | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Protective Sheathing | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Protective Sheathing | Mechanical Properties | High Strength | |
| Welded Tanks | Corrosion Resistance | Corrosion Resistance | |
| Welded Tanks | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Welded Tanks | Corrosion Resistance | Stress Corrosion Cracking Resistance | |
| Welded Tanks | Mechanical Properties | Moderate to High Strength | |
| Ordnance | Blending Chambers | Corrosion Resistance | Corrosion Resistance |
| Blending Chambers | Mechanical Properties | High Strength | |
| Blending Chambers | Non-Sparking | Non-Sparking | |
| Mixing Troughs | Corrosion Resistance | Corrosion Resistance | |
| Mixing Troughs | Mechanical Properties | High Strength | |
| Mixing Troughs | Non-Sparking | Non-Sparking |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Bolts | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Nuts | ASTM | F467 | NONFERROUS NUTS FOR GENERAL USE | ||
| Pipe | ASTM | B608 | WELDED COPPER ALLOY PIPE | ||
| Plate | ASTM | B100 | ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES | ||
| ASTM | B432 | COPPER AND COPPER ALLOY CLAD STEEL PLATE | |||
| FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | |||
| Plate & Sheet | for Pressure Vessels, Condensers & Heat Exchangers | ASTM | B171/B171M | COPPER ALLOY CONDENSER TUBE PLATES | |
| for Pressure Vessels, Condensers & Heat Exchangers | ASME | SB171 | COPPER ALLOY CONDENSER TUBE PLATES | ||
| Rod | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Rod, Bar & Shapes | for Pressure Vessels, Condensers & Heat Exchangers | ASTM | B150/B150M | ALUMINUM BRONZE ROD, BAR AND SHAPES | |
| for Pressure Vessels, Condensers & Heat Exchangers | ASME | SB150 | ALUMINUM BRONZE ROD, BAR, AND SHAPES | ||
| Screws | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Seamless Condenser Tube & Ferrule Stock | ASME | SB111 | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES & FERRULE STOCK | ||
| ASTM | B111/B111M | COPPER AND COPPER ALLOY SEAMLESS CONDENSER TUBES AND FERRULE STOCK | |||
| Seamless Pipe and Tube | ASTM | B315 | SEAMLESS COPPER ALLOY PIPE AND TUBE | ||
| ASME | SB315 | COPPER-SILICON ALLOY SEAMLESS PIPE AND TUBE | |||
| Shapes | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Sheet | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Sheet, Strip & Rolled Bar | Aluminum Bronze | ASME | SB169 | ALUMINUM BRONZE PLATE, SHEET, STRIP, AND ROLLED BAR | |
| Aluminum Bronze | ASTM | B169/B169M | ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND ROLLED BAR | ||
| Strip | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| FEDERAL | QQ-C-450 | COPPER-ALUMINUM ALLOY (ALUMINUM BRONZE, PLATE, SHEET, STRIP, AND BAR) | |||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Studs | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE |
Corrosion Properties