Find suppliers for this alloy
C61800
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | Al | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. |
||||||
| Min (%) | 0.50 | 8.5 | ||||
| Max (%) | Rem | 0.02 | 0.02 | 1.5 | 11.0 | 0.10 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||
| Rod | 1/2 Hard | H02 |
83 Typ |
39 Typ |
25 Typ |
88 Typ |
45 Typ |
2 | 15 | |
| 1/2 Hard | H02 |
80 Typ |
39 Typ |
28 Typ |
88 Typ |
43 Typ |
3 | 15 | ||
| 1/2 Hard | H02 |
85 Typ |
43 Typ |
23 Typ |
89 Typ |
47 Typ |
26 Typ | 1 | 15 | |
| Wire | 1/2 Hard | H02 |
140 Typ |
0.063 | ||||||
| 1/2 Hard | H02 |
125 Typ |
0.152 | |||||||
| Melting Point - Liquidus°F | 1913 |
|---|---|
| Melting Point - Solidus°F | 1904 |
| Densitylb/cu in. at 68°F | 0.272 |
| Specific Gravity | 7.53 |
| Electrical Conductivity% IACS at 68°F | 13 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 37 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Fair |
| Capacity for Being Hot Formed | Good |
| Forgeability Rating | 50 |
| Machinability Rating | 40 |
Common Fabrication Processes
- Drawing
- Hot forging
- Hot Pressing
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1100 | 1200 | ||
| Hot Working Temperature | 1400 | 1625 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Bearing Liners | Corrosion Resistance | Corrosion Resistance |
| Bearing Liners | Machining Characteristics | Average Speed | |
| Bearing Liners | Mechanical Properties | Medium Load | |
| Bearings | Corrosion Resistance | Corrosion Resistance | |
| Bearings | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Bearings | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Bearings | Friction & Wear Properties | Wear Resistance | |
| Bearings | Mechanical Properties | High Strength | |
| Bearings | Softening Resistance | Resistance to Softening | |
| Bushings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Bushings | Machining Characteristics | Average Speed | |
| Bushings | Mechanical Properties | Medium Load | |
| Pickling Hooks | Corrosion Resistance | Corrosion Resistance | |
| Pickling Hooks | Corrosion Resistance | Corrosion Resistance to Acids | |
| Pickling Hooks | Machining Characteristics | Average Speed | |
| Pickling Hooks | Mechanical Properties | Medium Load | |
| Pump Impellers | Corrosion Resistance | Corrosion Resistance | |
| Pump Impellers | Machining Characteristics | Average Speed | |
| Pump Impellers | Mechanical Properties | Medium Load | |
| Shafts | Corrosion Resistance | Corrosion Resistance | |
| Shafts | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Shafts | Mechanical Properties | High Strength | |
| Shafts | Softening Resistance | Resistance to Softening | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance in Numerous Environments | |
| Tie Rods | Mechanical Properties | High Strength | |
| Tie Rods | Softening Resistance | Resistance to Softening | |
| Welding Rod | Conductivity (Electrical) | Electrical Conductivity | |
| Welding Rod | Conductivity (Thermal) | Thermal Conductivity | |
| Welding Rod | Welding Characteristics | Weld to other Cu Al alloys | |
| Welding Wire | Welding Characteristics | Weld Alloy - c61300 | |
| Marine | Marine Hardware | Corrosion Resistance | Corrosion Resistance |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
| Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Marine Hardware | Mechanical Properties | Moderate Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Electrode | Welding | AWS | A5.6 | COPPER AND COPPER ALLOY COVERED ELECTRODES | |
| Rod | Welding | AWS | A5.13 | SURFACE WELDING RODS AND ELECTRODES | |
| Welding | AWS | A5.7 | COPPER AND COPPER ALLOY BARS, WELDING RODS | ||
| Welding | AWS | A5.15 | WELDING RODS FOR WELDING CAST IRON | ||
| Wire | AWS | A5.7 | COPPER AND COPPER ALLOY BARS, WELDING RODS | ||
| MILITARY | MIL-W-6712 | WIRE, METALLIZING |
Corrosion Properties