Find suppliers for this alloyC61800
Chemical Composition
Element
Cu(1,2)PbZnFeAlSi
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag.
Min (%)0.508.5
Max (%)Rem0.020.021.511.00.10
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Rod1/2 HardH0283   Typ
39   Typ
25   Typ
88   Typ
45   Typ
215
H0280   Typ
39   Typ
28   Typ
88   Typ
43   Typ
315
H0285   Typ
43   Typ
23   Typ
89   Typ
47   Typ
28   Typ
26   Typ
115
Wire1/2 HardH02140   Typ
0.063
H02125   Typ
0.152
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1913
Melting Point - Solidus°F1904
Densitylb/cu in. at 68°F0.272
Specific Gravity7.53
Electrical Conductivity% IACS at 68°F13
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F37
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingFair
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Spot WeldGood
Seam WeldGood
Butt WeldGood
Capacity for Being Cold WorkedFair
Capacity for Being Hot FormedGood
Forgeability Rating50
Machinability Rating40
Common Fabrication Processes
  • Drawing
  • Hot forging
  • Hot Pressing
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing11001200
Hot Treatment14001625
Typical uses
Product Category Product Reason Category Reason
IndustrialBearing LinersCorrosion ResistanceCorrosion Resistance
Bearing LinersMachining CharacteristicsAverage Speed
Bearing LinersMechanical PropertiesMedium Load
BearingsCorrosion ResistanceCorrosion Resistance
BearingsCorrosion ResistanceCorrosion Resistance in Numerous Environments
BearingsCorrosion ResistanceCorrosion Resistance to Chemicals
BearingsFriction & Wear PropertiesWear Resistance
BearingsMechanical PropertiesHigh Strength
BearingsSoftening ResistanceResistance to Softening
BushingsCorrosion ResistanceCorrosion Resistance (Excellent)
BushingsMachining CharacteristicsAverage Speed
BushingsMechanical PropertiesMedium Load
Pickling HooksCorrosion ResistanceCorrosion Resistance
Pickling HooksCorrosion ResistanceCorrosion Resistance to Acids
Pickling HooksMachining CharacteristicsAverage Speed
Pickling HooksMechanical PropertiesMedium Load
Pump ImpellersCorrosion ResistanceCorrosion Resistance
Pump ImpellersMachining CharacteristicsAverage Speed
Pump ImpellersMechanical PropertiesMedium Load
ShaftsCorrosion ResistanceCorrosion Resistance
ShaftsCorrosion ResistanceCorrosion Resistance in Numerous Environments
ShaftsMechanical PropertiesHigh Strength
ShaftsSoftening ResistanceResistance to Softening
Tie RodsCorrosion ResistanceCorrosion Resistance
Tie RodsCorrosion ResistanceCorrosion Resistance in Numerous Environments
Tie RodsMechanical PropertiesHigh Strength
Tie RodsSoftening ResistanceResistance to Softening
Welding RodConductivity (Electrical)Electrical Conductivity
Welding RodConductivity (Thermal)Thermal Conductivity
Welding RodWelding CharacteristicsWeld to other Cu Al alloys
Welding WireWelding CharacteristicsWeld Alloy - c61300
MarineMarine HardwareCorrosion ResistanceCorrosion Resistance
Marine HardwareCorrosion ResistanceCorrosion Resistance (Excellent)
Marine HardwareCorrosion ResistanceCorrosion Resistance to Salt Water
Marine HardwareMechanical PropertiesModerate Strength
Applicable Specifications
Form Specific Sub-Form Application System Standard Description
ElectrodeWeldingAWSA5.6COPPER AND COPPER ALLOY COVERED ELECTRODES
RodWeldingAWSA5.13SURFACE WELDING RODS AND ELECTRODES
WeldingAWSA5.15WELDING RODS FOR WELDING CAST IRON
WeldingAWSA5.7COPPER AND COPPER ALLOY BARS, WELDING RODS
WireAWSA5.7COPPER AND COPPER ALLOY BARS, WELDING RODS
MetallizingMILITARYMIL-W-6712WIRE, METALLIZING
Corrosion Properties