Chemical Composition
Element
Cu(1,2)SnFeNi(3)AlMnSi
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni value includes Co.
Min (%)2.08.5
Max (%)Rem0.64.01.010.00.500.25
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Shear Strength
(ksi)
Torsion Modulus
(ksi)
Izod
(ft-lbs)
Fatigue Strength**
(ksi)
Section Size
(in)
Cold Work
(%)
Bar1/2 HardH0290   Typ
45   Typ
30   Typ
85   Typ
115
H0285   Typ
40   Typ
30   Typ
82   Typ
215
As Hot ExtrudedM3075   Typ
35   Typ
35   Typ
80   Typ
3
Rod1/2 HardH0298   Typ
52   Typ
22   Typ
89   Typ
52   Typ
31   Typ
0.515
H0295   Typ
50   Typ
25   Typ
88   Typ
50   Typ
30   Typ
115
H0292   Typ
48   Typ
28   Typ
87   Typ
48   Typ
30   Typ
215
H0287   Typ
45   Typ
35   Typ
85   Typ
46   Typ
6.4   Typ
32   Typ
29   Typ
315
As Hot ExtrudedM3075   Typ
35   Typ
35   Typ
80   Typ
35   Typ
25   Typ
4
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1915
Melting Point - Solidus°F1905
Densitylb/cu in. at 68°F0.277
Specific Gravity7.67
Electrical Conductivity% IACS at 68°F12
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F31
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi17000
Modulus of Rigidityksi6400
Fabrication Properties
Technique Suitability
SolderingNot Recommended
BrazingFair
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingGood
Coated Metal Arc WeldingGood
Spot WeldGood
Seam WeldGood
Butt WeldGood
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedGood
Forgeability Rating75
Machinability Rating50
Common Fabrication Processes
  • Bending
  • Forging
  • Hot forging
  • Hot Pressing
  • Welding
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing11001200
Hot Treatment13001600
Typical uses
Product Category Product Reason Category Reason
FastenersBoltsCorrosion ResistanceCorrosion Resistance
BoltsCorrosion ResistanceCorrosion Resistance to Chemicals
BoltsCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
BoltsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BoltsMechanical PropertiesHigh Strength
NutsCorrosion ResistanceCorrosion Resistance to Chemicals
NutsCorrosion ResistanceCorrosion Resistance to Fresh Water
NutsCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
NutsCorrosion ResistanceCorrosion Resistance to Numerous Environments
NutsCorrosion ResistanceCorrosion Resistance to Salt Water
NutsMechanical PropertiesHigh Strength
IndustrialBearing RacesCorrosion ResistanceCorrosion Resistance
Bearing RacesFriction & Wear PropertiesMedium Wear Service
BearingsCorrosion ResistanceCorrosion Resistance
BearingsFriction & Wear PropertiesWear Resistance
BearingsMechanical PropertiesHigh Strength
BushingsCorrosion ResistanceCorrosion Resistance
BushingsFriction & Wear PropertiesMedium Wear Service
BushingsFriction & Wear PropertiesWear Resistance
BushingsMechanical PropertiesHigh Strength
CamsCorrosion ResistanceCorrosion Resistance
CamsCorrosion ResistanceCorrosion Resistance to Chemicals
CamsCorrosion ResistanceCorrosion Resistance to Fresh Water
CamsCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
CamsCorrosion ResistanceCorrosion Resistance to Numerous Environments
CamsCorrosion ResistanceCorrosion Resistance to Salt Water
CamsFriction & Wear PropertiesWear Resistance
CamsMechanical PropertiesHigh Strength
GearsCorrosion ResistanceCorrosion Resistance
GearsFriction & Wear PropertiesMedium Wear Service
GearsFriction & Wear PropertiesWear Resistance
GearsMechanical PropertiesHigh Strength
Pump RodsCorrosion ResistanceCorrosion Resistance
Pump RodsCorrosion ResistanceCorrosion Resistance to Chemicals
Pump RodsCorrosion ResistanceCorrosion Resistance to Fresh Water
Pump RodsCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
Pump RodsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Pump RodsCorrosion ResistanceCorrosion Resistance to Salt Water
Pump RodsFriction & Wear PropertiesGalling Resistance
Pump RodsFriction & Wear PropertiesWear Resistance
Pump RodsMechanical PropertiesHigh Strength
Valve GuidesCorrosion ResistanceCorrosion Resistance
Valve GuidesCorrosion ResistanceCorrosion Resistance to Chemicals
Valve GuidesCorrosion ResistanceCorrosion Resistance to Fresh Water
Valve GuidesCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
Valve GuidesCorrosion ResistanceCorrosion Resistance to Numerous Environments
Valve GuidesCorrosion ResistanceCorrosion Resistance to Salt Water
Valve GuidesFriction & Wear PropertiesGalling Resistance
Valve GuidesFriction & Wear PropertiesWear Resistance
Valve GuidesMechanical PropertiesHigh Strength
Valve SeatsCorrosion ResistanceCorrosion Resistance
Valve SeatsCorrosion ResistanceCorrosion Resistance to Chemicals
Valve SeatsCorrosion ResistanceCorrosion Resistance to Fresh Water
Valve SeatsCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
Valve SeatsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Valve SeatsCorrosion ResistanceCorrosion Resistance to Salt Water
Valve SeatsFriction & Wear PropertiesWear Resistance
Valve SeatsMechanical PropertiesHigh Strength
Valve StemsCorrosion ResistanceCorrosion Resistance
Valve StemsFriction & Wear PropertiesMedium Wear Service
Worm GearsCorrosion ResistanceCorrosion Resistance
Worm GearsCorrosion ResistanceCorrosion Resistance to Chemicals
Worm GearsCorrosion ResistanceCorrosion Resistance to Fresh Water
Worm GearsCorrosion ResistanceCorrosion Resistance to Non Oxidizing Acids
Worm GearsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Worm GearsCorrosion ResistanceCorrosion Resistance to Salt Water
Worm GearsFriction & Wear PropertiesWear Resistance
Worm GearsMechanical PropertiesHigh Strength
MarineMarine HardwareCorrosion ResistanceCorrosion Resistance not as good as C62200
Marine HardwareFriction & Wear PropertiesNon-Galling when run against Stainless Steel
Marine HardwareMechanical PropertiesHigher Strength than C62200
Applicable Specifications
Form Sub-Form System Standard Description
BarAMS4635ALUMINUM BRONZE BARS, RODS, AND FORGINGS, STRESS RELIEVED
ASMESB150ALUMINUM BRONZE ROD, BAR, AND SHAPES
ASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
ASTMB150/B150MALUMINUM BRONZE ROD, BAR AND SHAPES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
DieForgingsAMS4635ALUMINUM BRONZE BARS, RODS, AND FORGINGS, STRESS RELIEVED
ForgingsASTMB283/B283MCOPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED)
ForgingsMILITARYMIL-B-16166BRONZE, ALUMINUM, FORGINGS, HEAT TREATED
ForgingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
ForgingsSAEJ463WROUGHT COPPER AND COPPER ALLOYS
RodAMS4635ALUMINUM BRONZE BARS, RODS, AND FORGINGS, STRESS RELIEVED
ASMESB150ALUMINUM BRONZE ROD, BAR, AND SHAPES
ASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
ASTMB150/B150MALUMINUM BRONZE ROD, BAR AND SHAPES
SAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ShapesASTMB124/B124MCOPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES
ASTMB150/B150MALUMINUM BRONZE ROD, BAR AND SHAPES
Corrosion Properties

No information available.