Find suppliers for this alloy
C62400
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1,2) | Sn | Fe | Al | Mn | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
||||||
| Min (%) | 2.0 | 10.0 | ||||
| Max (%) | Rem | 0.20 | 4.5 | 11.5 | 0.30 | 0.25 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Izod (ft-lbs) |
Compressive Yield Strength (ksi) |
Fatigue Strength** (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
| Bar | As Hot Extruded | M30 |
90 Typ |
40 Typ |
18 Typ |
87 Typ |
3 | |||||||
| Light Anneal | O50 |
100 Typ |
50 Typ |
14 Typ |
92 Typ |
1 | ||||||||
| Light Anneal | O50 |
93 Typ |
45 Typ |
14 Typ |
91 Typ |
2 | ||||||||
| Rod | 1/2 Hard | H02 |
95 Typ |
47 Typ |
14 Typ |
91 Typ |
6.4 Typ | 17 Typ | 68 Typ | 34 Typ | 60 Typ |
3 | 10 | |
| 1/2 Hard | H02 |
105 Typ |
52 Typ |
14 Typ |
92 Typ |
65 Typ |
36 Typ | 1 | 10 | |||||
| 1/2 Hard | H02 |
95 Typ |
48 Typ |
14 Typ |
92 Typ |
62 Typ |
34 Typ | 2 | 10 | |||||
| As Hot Extruded | M30 |
90 Typ |
40 Typ |
18 Typ |
87 Typ |
58 Typ |
32 Typ | 4 | ||||||
| Melting Point - Liquidus°F | 1900 |
|---|---|
| Melting Point - Solidus°F | 1880 |
| Densitylb/cu in. at 68°F | 0.269 |
| Specific Gravity | 7.45 |
| Electrical Conductivity% IACS at 68°F | 12 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 34 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Not Recommended |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Good |
| Coated Metal Arc Welding | Good |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Poor |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 80 |
| Machinability Rating | 50 |
Common Fabrication Processes
- Hot bending
- Hot forging
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 1100 | 1200 | ||
| Hot Working Temperature | 1400 | 1625 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Fasteners | Nuts | Corrosion Resistance | Corrosion Resistance |
| Nuts | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Nuts | Mechanical Properties | High Strength | |
| Industrial | Bushings | Corrosion Resistance | Corrosion Resistance |
| Bushings | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | High Strength | |
| Cams | Corrosion Resistance | Corrosion Resistance | |
| Cams | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Cams | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Cams | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Cams | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Cams | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Cams | Friction & Wear Properties | Wear Resistance | |
| Cams | Mechanical Properties | High Strength | |
| Drift Pins | Corrosion Resistance | Corrosion Resistance | |
| Drift Pins | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Drift Pins | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Drift Pins | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Drift Pins | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Drift Pins | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Drift Pins | Impact Resistance | Impact Resistant | |
| Drift Pins | Mechanical Properties | High Strength | |
| Gears | Corrosion Resistance | Corrosion Resistance | |
| Gears | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Gears | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Gears | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Gears | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Gears | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Mechanical Properties | High Strength | |
| Hydraulic Bushings | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Bushings | Friction & Wear Properties | Resistant to Abrasive Wear | |
| Hydraulic Bushings | Impact Resistance | Impact Resistant | |
| Hydraulic Bushings | Mechanical Properties | High Strength | |
| Support Bushings | Friction & Wear Properties | Galling Resistance | |
| Support Bushings | Mechanical Properties | High Strength | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Chemicals | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Non Oxidizing Acids | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Tie Rods | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Tie Rods | Mechanical Properties | High Strength | |
| Valve Balls | Corrosion Resistance | Cavitation Corrosion Resistance | |
| Valve Balls | Corrosion Resistance | Erosion Corrosion Resistance | |
| Valve Balls | Corrosion Resistance | Pitting Corrosion Resistance | |
| Valve Balls | Corrosion Resistance | Resistance to Corrosion by a broad variety of Corrosive Media | |
| Valve Balls | Finishing Characteristics | Retains Surface Finish | |
| Valve Balls | Friction & Wear Properties | Wear Resistance | |
| Wear Plates | Corrosion Resistance | Corrosion Resistance | |
| Wear Plates | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
| Wear Plates | Friction & Wear Properties | Galling Resistance | |
| Wear Plates | Friction & Wear Properties | Wear Resistance | |
| Wear Plates | Mechanical Properties | High Strength | |
| Welding Wire | Conductivity (Electrical) | Electrical Conductivity | |
| Welding Wire | Conductivity (Thermal) | Thermal Conductivity | |
| Welding Wire | Corrosion Resistance | Oxidation Resistance | |
| Welding Wire | Softening Resistance | Resistance to Thermal Softening |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Forgings | Forgings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Forgings | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Rod | Welding | AWS | A5.7 | COPPER AND COPPER ALLOY BARS, WELDING RODS | |
| Rod, Bar & Shapes | Aluminum Bronze | ASTM | B150/B150M | ALUMINUM BRONZE ROD, BAR AND SHAPES | |
| Aluminum Bronze | ASME | SB150 | ALUMINUM BRONZE ROD, BAR, AND SHAPES |
Corrosion Properties