Find suppliers for this alloyC63600
Chemical Composition
Element
Cu(1,2)PbSnZnFeNi(3)AlAsSi
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni value includes Co.
Min (%)3.00.7
Max (%)Rem0.050.200.500.150.154.00.151.3
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
Elongation
(%)
Rockwell B scale
Section Size
(in)
Cold Work
(%)
Rod1/4 HardH0174   Typ
31   Typ
0.55
AnnealedO6160   Typ
64   Typ
Wire1/4 HardH0184   Typ
29   Typ
84   Typ
0.48821
1/8 HardH0068   Typ
52   Typ
71   Typ
0.4227
AnnealedO6160   Typ
67   Typ
0.392
* Measured at room temperature, 68°F (20°C).
Physical Properties
Melting Point - Liquidus°F1890
Densitylb/cu in. at 68°F0.301
Specific Gravity8.33
Electrical Conductivity% IACS at 68°F12
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F33
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)9.4
Modulus of Elasticity in Tensionksi16000
Fabrication Properties
Technique Suitability
SolderingNot Recommended
BrazingNot Recommended
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingFair
Spot WeldFair
Seam WeldFair
Butt WeldFair
Capacity for Being Cold WorkedExcellent
Capacity for Being Hot FormedFair
Machinability Rating40
Common Fabrication Processes
  • Cold Heading
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Hot Treatment14001600
Typical uses
Product Category Product Reason Category Reason
ElectricalCable ConnectorsConductivity (Electrical)Electrical Conductivity
Cable ConnectorsConductivity (Thermal)High Thermal Conductivity
Cable ConnectorsCorrosion ResistanceCorrosion Resistance
Cable ConnectorsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Cable ConnectorsMechanical PropertiesHigh Strength
Cold Headed NutsConductivity (Electrical)Electrical Conductivity
Cold Headed NutsConductivity (Thermal)High Thermal Conductivity
Cold Headed NutsCorrosion ResistanceCorrosion Resistance
Cold Headed NutsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Components for Pole Line HardwareConductivity (Electrical)Electrical Conductivity
Components for Pole Line HardwareConductivity (Thermal)High Thermal Conductivity
Components for Pole Line HardwareCorrosion ResistanceCorrosion Resistance
Components for Pole Line HardwareCorrosion ResistanceCorrosion Resistance to Numerous Environments
Components for Pole Line HardwareMachining PropertiesMachinability, Good
Components for Pole Line HardwareMechanical PropertiesHigh Strength
FastenersBoltsCorrosion ResistanceCorrosion Resistance
BoltsCorrosion ResistanceCorrosion Resistance to Numerous Environments
BoltsMechanical PropertiesHigh Strength
Screw Machine ProductsCorrosion ResistanceCorrosion Resistance
Screw Machine ProductsCorrosion ResistanceCorrosion Resistance to Numerous Environments
Screw Machine ProductsMechanical PropertiesModerate Strength
IndustrialValve Components, Nuclear Power ServiceCorrosion ResistanceCorrosion Resistance to Uranium Hexafloride
Valve Components, Nuclear Power ServiceForging CharacteristicsForgability
Valve Components, Nuclear Power ServiceMechanical PropertiesModerate Strength
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.