Find suppliers for this alloy
C64400
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1) | Pb | Sn | Zn | Fe | Ni(2) | Al | Si | |
|
(1) Cu value includes Ag. (2) Ni value includes Co. |
||||||||
| Min (%) | 4.2 | 3.5 | 0.8 | |||||
| Max (%) | Rem | 0.03 | 0.10 | 0.20 | 0.05 | 5.0 | 4.5 | 1.3 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell 30T scale | Fatigue Strength** (ksi) |
|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||
| Sheet | 1/2 Hard | H02 |
90 Typ |
75 Typ |
18 Typ |
76 Typ |
||
| 1/2 Hard and Precipitation Heat Treated | TH02 |
127 Typ |
118 Typ |
8 Typ |
83 Typ |
45 Typ | ||
| 1/4 Hard | H01 |
80 Typ |
56 Typ |
30 Typ |
68 Typ |
|||
| 1/4 Hard and Precipitation Heat Treated | TH01 |
110 Typ |
96 Typ |
21 Typ |
80 Typ |
44 Typ | ||
| Hard | H04 |
118 Typ |
100 Typ |
8 Typ |
80 Typ |
|||
| Hard and Precipitation Heat Treated | TH04 |
138 Typ |
131 Typ |
3 Typ |
85 Typ |
|||
| Precipitation Hardened | TF00 |
95 Typ |
75 Typ |
25 Typ |
73 Typ |
|||
| Soft Anneal | O60 |
70 Typ |
50 Typ |
37 Typ |
60 Typ |
|||
| Strip | 1/2 Hard | H02 |
90 Typ |
75 Typ |
18 Typ |
68 Typ |
||
| 1/2 Hard and Precipitation Heat Treated | TH02 |
127 Typ |
118 Typ |
8 Typ |
83 Typ |
45 Typ | ||
| 1/4 Hard | H01 |
80 Typ |
56 Typ |
30 Typ |
68 Typ |
|||
| 1/4 Hard and Precipitation Heat Treated | TH01 |
110 Typ |
96 Typ |
21 Typ |
80 Typ |
44 Typ | ||
| Hard | H04 |
118 Typ |
100 Typ |
8 Typ |
80 Typ |
|||
| Hard and Precipitation Heat Treated | TH04 |
138 Typ |
131 Typ |
3 Typ |
85 Typ |
|||
| Precipitation Hardened | TF00 |
95 Typ |
75 Typ |
25 Typ |
73 Typ |
|||
| Soft Anneal | O60 |
70 Typ |
50 Typ |
37 Typ |
60 Typ |
|||
| (1)As rolled condition. | |
| Melting Point - Liquidus°F | 1922 |
|---|---|
| Melting Point - Solidus°F | 1859 |
| Densitylb/cu in. at 68°F | 0.29 |
| Specific Gravity | 8.03 |
| Electrical Conductivity% IACS at 68°F | 20 (1) |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Fair |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Fair |
| Seam Weld | Fair |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
Common Fabrication Processes
- Drawing
- Forming
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Bellows | Corrosion Resistance | Corrosion Resistance |
| Bellows | Machining Properties | Machinability, Good | |
| Bellows | Mechanical Properties | High Strength | |
| Clips | Conductivity (Electrical) | Electrical Conductivity | |
| Clips | Conductivity (Thermal) | Thermal Conductivity | |
| Clips | Corrosion Resistance | Corrosion Resistance | |
| Clips | Mechanical Properties | High Strength | |
| Connectors | Conductivity (Electrical) | Electrical Conductivity | |
| Connectors | Conductivity (Thermal) | High Thermal Conductivity | |
| Connectors | Corrosion Resistance | Corrosion Resistance | |
| Connectors | Mechanical Properties | High Strength | |
| Contacts | Conductivity (Electrical) | Electrical Conductivity | |
| Contacts | Conductivity (Thermal) | Thermal Conductivity | |
| Contacts | Corrosion Resistance | Corrosion Resistance | |
| Contacts | Mechanical Properties | High Strength | |
| Diaphragms for Pressure Sensitive Contacts | Conductivity (Electrical) | Electrical Conductivity | |
| Diaphragms for Pressure Sensitive Contacts | Conductivity (Thermal) | High Thermal Conductivity | |
| Diaphragms for Pressure Sensitive Contacts | Corrosion Resistance | Corrosion Resistance | |
| Diaphragms for Pressure Sensitive Contacts | Mechanical Properties | High Strength | |
| Instrumentation | Conductivity (Electrical) | Electrical Conductivity | |
| Instrumentation | Conductivity (Thermal) | High Thermal Conductivity | |
| Instrumentation | Corrosion Resistance | Corrosion Resistance | |
| Instrumentation | Mechanical Properties | High Strength | |
| Safety Devices | Corrosion Resistance | Corrosion Resistance | |
| Safety Devices | Mechanical Properties | High Strength | |
| Safety Devices | Non-Sparking | Non-Sparking | |
| Springs | Corrosion Resistance | Corrosion Resistance | |
| Springs | Mechanical Properties | High Strength | |
| Switches | Conductivity (Electrical) | Electrical Conductivity | |
| Switches | Conductivity (Thermal) | High Thermal Conductivity | |
| Switches | Corrosion Resistance | Corrosion Resistance | |
| Switches | Mechanical Properties | High Strength |
Applicable Specifications
Corrosion Properties