C64770
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Mg | Mn | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. (3) Ni value includes Co. |
|||||||||
| Min (%) | 0.05 | 0.30 | 1.5 | 0.40 | |||||
| Max (%) | Rem | 0.05 | 0.50 | 0.8 | 0.10 | 3.0 | 0.30 | 0.10 | 0.8 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 3000 gm |
|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | ||||||
| Flat Products | 3/4 Hard | H03 |
87 Min 97 Typ 101 Max |
73 Min 80 Typ 87 Max |
15 Typ |
195 Typ |
| Extra Hard | H06 |
100 Min 107 Typ 115 Max |
90 Min 96 Typ 104 Max |
5 Typ |
225 Typ |
|
| Hard | H04 |
93 Min 100 Typ 107 Max |
80 Min 87 Typ 94 Max |
10 Typ |
205 Typ |
|
| Spring | H08 |
107 Min 113 Typ 122 Max |
102 Min 109 Typ 116 Max |
1 Typ |
235 Typ |
|
| Melting Point - Solidus°F | 1967 |
|---|---|
| Densitylb/cu in. at 68°F | 0.318 |
| Specific Gravity | 8.79 |
| Electrical Conductivity% IACS at 68°F | 40 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 98 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 19200 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Not Recommended |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Not Recommended |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Not Recommended |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
Common Fabrication Processes
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Connectors, Automotive | ||
| Connectors, Electrical, Lead-Free | Conductivity (Electrical) | Electrical Conductivity | |
| Connectors, Electrical, Lead-Free | Conductivity (Thermal) | Thermal Conductivity | |
| Connectors, Electrical, Lead-Free | Corrosion Resistance | Corrosion Resistance | |
| Connectors, Electrical, Lead-Free | Corrosion Resistance | Stress corrosion resistance, high | |
| Connectors, Electrical, Lead-Free | Forming Characteristics | Formability | |
| Connectors, Electrical, Lead-Free | Plating Characteristics | Platability | |
| Connectors, electronic | |||
| Contact springs | |||
| Crcuit Breaker Components | Conductivity (Thermal) | Thermal Conductivity | |
| Crcuit Breaker Components | Corrosion Resistance | Resistance to Corrosion - General and Pitting in Water Radiators | |
| Crcuit Breaker Components | Solderability | Solderability | |
| Relay Components |
Applicable Specifications
Corrosion Properties