C64780
| Elements | |||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Ni | Cr | Mg | Mn | Si | Ti | Zr | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. |
|||||||||||
| Min (%) | 90.0 | 0.10 | 0.20 | 1.0 | 0.01 | 0.20 | |||||
| Max (%) | 0.02 | 2.0 | 2.5 | 3.5 | 0.01 | 0.01 | 1.0 | 0.9 | 0.01 | 0.01 | |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
Vickers Hardness, 500 gm | Fatigue Strength** (ksi) |
Proportional Limit (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||
| Flat Products | 1/2 Hard | H02 |
74 Typ |
65 Typ |
15 Typ |
160 Typ |
62 Typ | ||
| Extra Hard | H06 |
103 Typ |
94 Typ |
14 Typ |
225 Typ |
38 Typ | 77 Typ | 0.009 | |
| Extra Spring | H10 |
123 Typ |
113 Typ |
11 Typ |
255 Typ |
41 Typ | 88 Typ | ||
| Hard | H04 |
86 Typ |
78 Typ |
10 Typ |
185 Typ |
35 Typ | 70 Typ | ||
| Melting Point - Liquidus°F | 1989 |
|---|---|
| Melting Point - Solidus°F | 1954 |
| Densitylb/cu in. at 68°F | 0.321 |
| Specific Gravity | 8.9 |
| Electrical Conductivity% IACS at 68°F | 48 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 116.2 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.095 |
| Modulus of Elasticity in Tensionksi | 11600 |
| Modulus of Rigidityksi | 4400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Good |
| Gas Shielded Arc Welding | Good |
| Spot Weld | Good |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Good |
| Machinability Rating | 20 |
Common Fabrication Processes
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 842 | |||
| Hot Working Temperature | 1382 | 1832 | ||
| Stress Relief | 482 | |||