Find suppliers for this alloy
C65100
| Elements | ||||||
|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | Mn | Si | |
|
(1) Cu value includes Ag. (2) Cu + Sum of Named Elements 99.5% min. |
||||||
| Min (%) | 0.8 | |||||
| Max (%) | Rem | 0.05 | 1.5 | 0.8 | 0.7 | 2.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Fatigue Strength** (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
| Rod | Extra Hard | H06 |
90 Typ |
12 Typ |
90 Typ |
50 Typ |
1 | 50 | ||||||
| Hard | H04 |
70 Typ |
55 Typ |
15 Typ |
80 Typ |
45 Typ |
6.4 Typ | 28 Typ | 1 | 36 | ||||
| Nominal Grain Size 0.035 mm | OS035 |
40 Typ |
15 Typ |
50 Typ |
55 Typ |
1 | ||||||||
| Rod & Wire | Extra Hard | H06 |
105 Typ |
10 Typ |
53 Typ |
0.08 | ||||||||
| Extra Hard | H06 |
90 Typ |
67 Typ |
12 Typ |
50 Typ |
1 | 50 | |||||||
| Hard | H04 |
70 Typ |
55 Typ |
15 Typ |
45 Typ |
1 | 36 | |||||||
| Hard | H04 |
100 Typ |
70 Typ |
11 Typ |
50 Typ |
0.08 | ||||||||
| Hard | H04 |
95 Typ |
12 Typ |
0.44 | 60 | |||||||||
| Tube | Hard Drawn | H80 |
65 Typ |
20 Typ |
75 Typ |
67 Typ |
35 | |||||||
| Hard Drawn | H80 |
65 Typ |
40 Typ |
20 Typ |
35 | |||||||||
| Nominal Grain Size 0.015 mm | OS015 |
45 Typ |
20 Typ |
55 Typ |
68 Typ |
0.065 | ||||||||
| Wire | 1/2 Hard | H02 |
80 Typ |
15 Typ |
45 Typ |
0.08 | ||||||||
| 1/2 Hard | H02 |
80 Typ |
20 Typ |
0.44 | 37 | |||||||||
| 1/4 Hard | H01 |
63 Typ |
30 Typ |
0.44 | 21 | |||||||||
| 1/4 Hard | H01 |
65 Typ |
50 Typ |
25 Typ |
40 Typ |
0.08 | ||||||||
| 1/8 Hard | H00 |
55 Typ |
40 Typ |
40 Typ |
36 Typ |
0.08 | ||||||||
| 1/8 Hard | H00 | 30 Typ |
63 Typ |
0.44 | 21 | |||||||||
| 1/8 Hard | H00 |
55 Typ |
40 Typ |
40 Typ |
36 Typ |
0.08 | ||||||||
| Extra Hard | H06 |
105 Typ |
71 Typ |
10 Typ |
53 Typ |
28 Typ | 0.08 | |||||||
| Hard | H04 |
95 Typ |
12 Typ |
0.44 | 60 | |||||||||
| Hard | H04 |
100 Typ |
70 Typ |
11 Typ |
50 Typ |
25 Typ | 0.08 | |||||||
| Melting Point - Liquidus°F | 1940 |
|---|---|
| Melting Point - Solidus°F | 1890 |
| Densitylb/cu in. at 68°F | 0.316 |
| Specific Gravity | 8.75 |
| Electrical Conductivity% IACS at 68°F | 12 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 33 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.9 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Modulus of Rigidityksi | 6400 |
| Technique | Suitability |
|---|---|
| Soldering | Excellent |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Excellent |
| Seam Weld | Good |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Machinability Rating | 30 |
Common Fabrication Processes
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Roll Threading and Knurling
- Squeezing and Swaging
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 900 | 1250 | ||
| Hot Working Temperature | 1300 | 1300 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Electrical | Conduit | Conductivity (Electrical) | Electrical Conductivity |
| Conduit | Conductivity (Thermal) | Thermal Conductivity | |
| Conduit | Corrosion Resistance | Corrosion Resistance | |
| Conduit | Mechanical Properties | High Strength | |
| Conduit | Solderability | Solderability | |
| Motor, Rotor Bars | Brazing Characteristics | Brazability | |
| Motor, Rotor Bars | Conductivity (Electrical) | Electrical Resistivity | |
| Motor, Rotor Bars | Mechanical Properties | Moderate Strength | |
| Pole Line Hardware | Conductivity (Electrical) | Electrical Conductivity | |
| Pole Line Hardware | Corrosion Resistance | Corrosion Resistance | |
| Pole Line Hardware | Mechanical Properties | Moderate Strength | |
| Fasteners | Bolts | Corrosion Resistance | Corrosion Resistance |
| Bolts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Bolts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Bolts | Mechanical Properties | High Strength | |
| Cable Clamps | Corrosion Resistance | Corrosion Resistance | |
| Cable Clamps | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Cable Clamps | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Cable Clamps | Mechanical Properties | High Strength | |
| Cap Screws | Corrosion Resistance | Corrosion Resistance | |
| Cap Screws | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Cap Screws | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Cap Screws | Forming Characteristics | Excellent Formability | |
| Cap Screws | Mechanical Properties | High Strength | |
| Fasteners | Conductivity (Electrical) | Electrical Conductivity | |
| Fasteners | Corrosion Resistance | Corrosion Resistance | |
| Fasteners | Mechanical Properties | High Strength | |
| Machine Screws | Corrosion Resistance | Corrosion Resistance | |
| Machine Screws | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Machine Screws | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Machine Screws | Mechanical Properties | High Strength | |
| Nuts | Corrosion Resistance | Corrosion Resistance | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Nuts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Nuts | Mechanical Properties | High Strength | |
| Rivets | Corrosion Resistance | Corrosion Resistance | |
| Rivets | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Rivets | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Rivets | Forming Characteristics | Formability | |
| Rivets | Mechanical Properties | High Strength | |
| Screws | Corrosion Resistance | Corrosion Resistance | |
| Screws | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Screws | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Screws | Mechanical Properties | High Strength | |
| U Bolts | Corrosion Resistance | Corrosion Resistance | |
| U Bolts | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| U Bolts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| U Bolts | Mechanical Properties | High Strength | |
| Industrial | Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Heat Exchanger Tube | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Heat Exchanger Tube | Forming Characteristics | Excellent Formability | |
| Heat Exchanger Tube | Mechanical Properties | High Strength | |
| Heat Exchanger Tube | Welding Characteristics | Weldability | |
| Hydraulic Pressure Lines | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Pressure Lines | Forming Characteristics | Excellent Formability | |
| Hydraulic Pressure Lines | Mechanical Properties | High Strength | |
| Hydraulic Pressure Lines | Thermal Properties | Resistance to Stress Relaxation | |
| Hydraulic Pressure Lines | Welding Characteristics | Weldability | |
| Oil Refinery Plumbing Tube | Corrosion Resistance | Corrosion Resistance | |
| Oil Refinery Plumbing Tube | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Oil Refinery Plumbing Tube | Mechanical Properties | Moderate Strength | |
| Welding Rod | Conductivity (Electrical) | Electrical Conductivity | |
| Welding Rod | Conductivity (Thermal) | Thermal Conductivity | |
| Welding Rod | Corrosion Resistance | Oxidation Resistance | |
| Welding Rod | Softening Resistance | Resistance to Thermal Softening | |
| Marine | Hardware | Corrosion Resistance | Corrosion Resistance |
| Hardware | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Hardware | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bolts | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Nuts | ASTM | F467 | NONFERROUS NUTS FOR GENERAL USE | ||
| Plate | ASTM | B432 | COPPER AND COPPER ALLOY CLAD STEEL PLATE | ||
| Rod, Bar & Shapes | Copper-Silicon Alloy | ASTM | B98/B98M | COPPER-SILICON ALLOY ROD, BAR AND SHAPES | |
| Copper-Silicon Alloy | ASME | SB98 | COPPER-SILICON ALLOY ROD, BAR AND SHAPES | ||
| Screws | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Seamless Pipe and Tube | ASTM | B315 | SEAMLESS COPPER ALLOY PIPE AND TUBE | ||
| ASME | SB315 | COPPER-SILICON ALLOY SEAMLESS PIPE AND TUBE | |||
| Sheet, Strip, Roller Bar & Plate | for Pressure Vessels, Condensers & Heat Exchangers | ASTM | B96/B96M | COPPER SILICON ALLOY PLATE, SHEET, STRIP AND ROLLED BAR FOR GENERAL PURPOSES AND PRESSURE VESSELS | |
| for Pressure Vessels, Condensers & Heat Exchangers | ASME | SB96 | COPPER-SILICON ALLOY PLATE AND SHEET FOR PRESSURE VESSELS | ||
| Studs | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Wire | ASTM | B99/B99M | COPPER-SILICON ALLOY WIRE FOR GENERAL PURPOSES | ||
| ASTM | B105 | HARD-DRAWN COPPER ALLOY WIRES FOR ELECTRICAL CONDUCTORS |
Corrosion Properties