Find suppliers for this alloy
C65500
| Elements | |||||||
|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | Ni(3) | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. (3) Ni value includes Co. |
|||||||
| Min (%) | 0.50 | 2.8 | |||||
| Max (%) | Rem | 0.05 | 1.5 | 0.8 | 0.6 | 1.3 | 3.8 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Fatigue Strength** (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
Cold Work (%) |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
| Flat Products | 1/2 Hard | H02 |
78 Typ |
17 Typ |
87 Typ |
75 Typ |
50 Typ |
0.04 | ||||||
| 1/4 Hard | H01 |
68 Typ |
35 Typ |
30 Typ |
75 Typ |
67 Typ |
47 Typ |
0.04 | ||||||
| Extra Hard | H06 |
104 Typ |
60 Typ |
6 Typ |
96 Typ |
80 Typ |
60 Typ |
0.04 | ||||||
| Hard | H04 |
94 Typ |
58 Typ |
8 Typ |
93 Typ |
78 Typ |
57 Typ |
0.04 | ||||||
| Nominal Grain Size 0.015 mm | OS015 |
63 Typ |
30 Typ |
55 Typ |
66 Typ |
90 Typ |
45 Typ |
0.04 | ||||||
| Nominal Grain Size 0.035 mm | OS035 |
60 Typ |
25 Typ |
60 Typ |
62 Typ |
85 Typ |
43 Typ |
0.04 | ||||||
| Nominal Grain Size 0.070 mm | OS070 |
56 Typ |
21 Typ |
63 Typ |
40 Typ |
76 Typ |
42 Typ |
0.04 | ||||||
| Spring | H08 |
110 Typ |
62 Typ |
4 Typ |
97 Typ |
81 Typ |
63 Typ |
0.04 | ||||||
| Flat Products & Wire | Nominal Grain Size 0.035 mm | OS035 |
60 Typ |
60 Typ |
43 Typ |
0.08 | ||||||||
| Spring | H08 |
145 Typ |
70 Typ |
3 Typ |
70 Typ |
0.08 | 80 | |||||||
| Spring | H08 |
110 Typ |
62 Typ |
4 Typ |
63 Typ |
0.04 | ||||||||
| Flat Products, Rod & Bar | 1/2 Hard | H02 |
98 Typ |
8 Typ |
58 Typ |
0.08 | ||||||||
| 1/2 Hard | H02 |
78 Typ |
45 Typ |
35 Typ |
52 Typ |
1 | 20 | |||||||
| 1/2 Hard | H02 |
78 Typ |
45 Typ |
17 Typ |
50 Typ |
0.04 | ||||||||
| Rod | 1/2 Hard | H02 |
78 Typ |
35 Typ |
85 Typ |
52 Typ |
1 | 20 | ||||||
| Extra Hard | H06 |
108 Typ |
60 Typ |
13 Typ |
95 Typ |
5.7 Typ | 62 Typ |
1 | 50 | |||||
| Hard | H04 |
92 Typ |
55 Typ |
22 Typ |
90 Typ |
58 Typ |
30 Typ | 1 | 36 | |||||
| Nominal Grain Size 0.050 mm | OS050 |
58 Typ |
22 Typ |
60 Typ |
60 Typ |
43 Typ |
1 | |||||||
| Rod & Tubing | Nominal Grain Size 0.050 mm | OS050 |
58 Typ |
60 Typ |
43 Typ |
1 | ||||||||
| Nominal Grain Size 0.050 mm | OS050 |
57 Typ |
70 Typ |
|||||||||||
| Tube | Hard Drawn | H80 |
93 Typ |
22 Typ |
92 Typ |
78 Typ |
0.065 | 35 | ||||||
| Nominal Grain Size 0.050 mm | OS050 |
57 Typ |
70 Typ |
45 Typ |
0.065 | |||||||||
| Wire | 1/2 Hard | H02 |
98 Typ |
8 Typ |
58 Typ |
0.08 | ||||||||
| 1/4 Hard | H01 |
80 Typ |
48 Typ |
20 Typ |
52 Typ |
0.08 | ||||||||
| 1/8 Hard | H00 |
70 Typ |
40 Typ |
35 Typ |
48 Typ |
0.08 | ||||||||
| Hard | H04 |
125 Typ |
65 Typ |
5 Typ |
65 Typ |
29 Typ | 0.08 | |||||||
| Nominal Grain Size 0.035 mm | OS035 |
60 Typ |
25 Typ |
60 Typ |
43 Typ |
0.08 | ||||||||
| Spring | H08 |
145 Typ |
70 Typ |
3 Typ |
70 Typ |
30 Typ | 0.08 | |||||||
| Melting Point - Liquidus°F | 1880 |
|---|---|
| Melting Point - Solidus°F | 1780 |
| Densitylb/cu in. at 68°F | 0.308 |
| Specific Gravity | 8.53 |
| Electrical Conductivity% IACS at 68°F | 7 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 21 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 15000 |
| Modulus of Rigidityksi | 5600 |
| Technique | Suitability |
|---|---|
| Soldering | Good |
| Brazing | Excellent |
| Oxyacetylene Welding | Good |
| Gas Shielded Arc Welding | Excellent |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Excellent |
| Seam Weld | Excellent |
| Butt Weld | Excellent |
| Capacity for Being Cold Worked | Excellent |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 40 |
| Machinability Rating | 30 |
Common Fabrication Processes
- Blanking
- Drawing
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Roll Threading and Knurling
- Shearing
- Squeezing and Swaging
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 900 | 1300 | ||
| Hot Working Temperature | 1300 | 1600 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Consumer | Sculpture | Appearance | Appearance |
| Sculpture | Corrosion Resistance | Corrosion Resistance | |
| Sculpture | Welding Characteristics | Weldability | |
| Electrical | Motors, Rotor Bar | Brazing Characteristics | Brazability |
| Motors, Rotor Bar | Conductivity (Electrical) | Electrical Resistivity | |
| Pole Line Hardware | Conductivity (Electrical) | Electrical Conductivity | |
| Pole Line Hardware | Conductivity (Thermal) | Thermal Conductivity | |
| Pole Line Hardware | Corrosion Resistance | Corrosion Resistance | |
| Pole Line Hardware | Mechanical Properties | High Strength | |
| Fasteners | Bolts | Corrosion Resistance | Corrosion Resistance |
| Bolts | Mechanical Properties | High Strength | |
| Burrs | Corrosion Resistance | Corrosion Resistance | |
| Burrs | Mechanical Properties | High Strength | |
| Clamps | Corrosion Resistance | Corrosion Resistance | |
| Clamps | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Clamps | Mechanical Properties | High Strength | |
| Cotter Pins | Corrosion Resistance | Corrosion Resistance | |
| Cotter Pins | Mechanical Properties | High Strength | |
| Hinges | Corrosion Resistance | Corrosion Resistance | |
| Hinges | Mechanical Properties | High Strength | |
| Nails | Corrosion Resistance | Corrosion Resistance | |
| Nails | Mechanical Properties | High Strength | |
| Nuts | Corrosion Resistance | Corrosion Resistance | |
| Nuts | Mechanical Properties | High Strength | |
| Rivets | Appearance | Appearance | |
| Rivets | Corrosion Resistance | Corrosion Resistance | |
| Rivets | Forming Characteristics | Formability | |
| Rivets | Mechanical Properties | High Strength | |
| Screws | Corrosion Resistance | Corrosion Resistance | |
| Screws | Mechanical Properties | High Strength | |
| Industrial | Bearing Plates | Corrosion Resistance | Corrosion Resistance |
| Bearing Plates | Friction & Wear Properties | Galling Resistance | |
| Bearing Plates | Friction & Wear Properties | Wear Resistance | |
| Bearing Plates | Mechanical Properties | High Strength | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Mechanical Properties | High Strength | |
| Butts | Corrosion Resistance | Corrosion Resistance | |
| Butts | Mechanical Properties | High Strength | |
| Cable | Corrosion Resistance | Corrosion Resistance | |
| Cable | Forming Characteristics | Formability | |
| Cable | Mechanical Properties | High Strength | |
| Channels | Corrosion Resistance | Corrosion Resistance | |
| Channels | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Channels | Corrosion Resistance | Corrosion Resistance to Paper Industry Chemicals | |
| Channels | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Channels | Forming Characteristics | Formability | |
| Channels | Mechanical Properties | High Strength | |
| Channels | Non-Sparking | Non-Sparking | |
| Channels | Welding Characteristics | Weldability | |
| Chemical Equipment | Corrosion Resistance | Corrosion Resistance | |
| Chemical Equipment | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Chemical Equipment | Mechanical Properties | High Strength | |
| Chemical Equipment | Welding Characteristics | Weldability | |
| Doctor Blades, Paper Industry | Corrosion Resistance | Corrosion Resistance | |
| Doctor Blades, Paper Industry | Corrosion Resistance | Corrosion Resistance to Paper Industry Chemicals | |
| Doctor Blades, Paper Industry | Friction & Wear Properties | Wear Resistance | |
| Doctor Blades, Paper Industry | Mechanical Properties | Moderate to High Strength | |
| Heat Exchanger Tubes | Corrosion Resistance | Corrosion Resistance | |
| Heat Exchanger Tubes | Forming Characteristics | Formability | |
| Heat Exchanger Tubes | Mechanical Properties | High Strength | |
| Heat Exchanger Tubes | Solderability | Solderability | |
| Heat Exchanger Tubes | Welding Characteristics | Weldability | |
| Hydraulic Pressure Lines | Corrosion Resistance | Corrosion Resistance | |
| Hydraulic Pressure Lines | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Hydraulic Pressure Lines | Mechanical Properties | High Strength | |
| Hydraulic Pressure Lines | Welding Characteristics | Weldability | |
| Kettles | Corrosion Resistance | Corrosion Resistance | |
| Kettles | Corrosion Resistance | Corrosion Resistance to Paper Industry Chemicals | |
| Kettles | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Kettles | Mechanical Properties | High Strength | |
| Oil Refinery Plumbing Tube | Corrosion Resistance | Corrosion Resistance | |
| Oil Refinery Plumbing Tube | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Oil Refinery Plumbing Tube | Mechanical Properties | Moderate to High Strength | |
| Oil Refinery Plumbing Tube | Non-Sparking | Non-Sparking | |
| Oil Refinery Plumbing Tube | Welding Characteristics | Weldability | |
| Piston Rings | Corrosion Resistance | Corrosion Resistance | |
| Piston Rings | Friction & Wear Properties | Wear Resistance | |
| Piston Rings | Mechanical Properties | High Strength | |
| Pressure Vessels | Corrosion Resistance | Corrosion Resistance | |
| Pressure Vessels | Welding Characteristics | Weldability | |
| Screen Cloth | Corrosion Resistance | Corrosion Resistance | |
| Screen Cloth | Forming Characteristics | Formability | |
| Screen Cloth | Mechanical Properties | High Strength | |
| Screen Plates | Corrosion Resistance | Corrosion Resistance | |
| Screen Plates | Forming Characteristics | Formability | |
| Screen Plates | Mechanical Properties | High Strength | |
| Shafting | Corrosion Resistance | Corrosion Resistance | |
| Shafting | Mechanical Properties | High Strength | |
| Shafting | Welding Characteristics | Weldability | |
| Tanks | Corrosion Resistance | Corrosion Resistance | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Petrochemicals | |
| Tanks | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Tanks | Mechanical Properties | High Strength | |
| Wear Plates | Friction & Wear Properties | Galling Resistance | |
| Wear Plates | Friction & Wear Properties | Wear Resistance | |
| Welded Pressure Vessels | Corrosion Resistance | Corrosion Resistance | |
| Welded Pressure Vessels | Welding Characteristics | Weldability | |
| Welded Tanks | Corrosion Resistance | Corrosion Resistance | |
| Welded Tanks | Welding Characteristics | Weldability | |
| Wire | Corrosion Resistance | Corrosion Resistance | |
| Wire | Mechanical Properties | High Strength | |
| Marine | Hardware | Appearance | Appearance |
| Hardware | Corrosion Resistance | Corrosion Resistance | |
| Hardware | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
| Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Hardware | Mechanical Properties | High Strength | |
| Propeller Shafts | Corrosion Resistance | Corrosion Resistance | |
| Propeller Shafts | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Propeller Shafts | Friction & Wear Properties | Wear Resistance | |
| Propeller Shafts | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Bolts | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Forgings, Die (Hot Pressed) | ASME | SB283 | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | ||
| ASTM | B283/B283M | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | |||
| Nuts | ASTM | F467 | NONFERROUS NUTS FOR GENERAL USE | ||
| Plate | Bridge and Bearing | ASTM | B100 | ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES | |
| Rod | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Forgings | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Rod, Bar & Shapes | Copper-Silicon Alloy | ASTM | B98/B98M | COPPER-SILICON ALLOY ROD, BAR AND SHAPES | |
| Copper-Silicon Alloy | ASME | SB98 | COPPER-SILICON ALLOY ROD, BAR AND SHAPES | ||
| Screws | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Seamless Pipe and Tube | ASTM | B315 | SEAMLESS COPPER ALLOY PIPE AND TUBE | ||
| ASME | SB315 | COPPER-SILICON ALLOY SEAMLESS PIPE AND TUBE | |||
| Shapes | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Forgings | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Sheet | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Bridge and Bearing | ASTM | B100 | ROLLED COPPER ALLOY BEARING AND EXPANSION PLATES AND SHEETS FOR BRIDGE AND OTHER STRUCTURAL USES | ||
| Sheet, Strip, Roller Bar & Plate | for Pressure Vessels & General Purpose | ASTM | B96/B96M | COPPER SILICON ALLOY PLATE, SHEET, STRIP AND ROLLED BAR FOR GENERAL PURPOSES AND PRESSURE VESSELS | |
| for Pressure Vessels & General Purpose | ASME | SB96 | COPPER-SILICON ALLOY PLATE AND SHEET FOR PRESSURE VESSELS | ||
| Strip | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Studs | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
| Tube | MILITARY | MIL-T-8231 | TUBES: COPPER-SILICON-BRONZE, SEAMLESS, FOR AIRCRAFT | ||
| Wire | ASTM | B99/B99M | COPPER-SILICON ALLOY WIRE FOR GENERAL PURPOSES |
Corrosion Properties