Find suppliers for this alloyC66910
Chemical Composition
Element
Cu(1,2)PbSnZnFeNiAlCoMnTiZrNb
(1) Not including Ag. (2) Cu + Sum of Named Elements 99.5% min.
Min (%)6.00.010.0112.0
Max (%)Rem0.050.058.01.53.50.250.0115.00.150.150.05
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
Flat Products & Tubing1/2 HardH0284   Typ
1/4 HardH0175   Typ
AnnealANNEAL67   Typ
Extra HardH06108   Typ
HardH0492   Typ
SpringH08118   Typ
* Measured at room temperature, 68°F (20°C).
Physical Properties
(1) As annealed
Densitylb/cu in. at 68°F0.298
Specific Gravity8.25
Electrical Conductivity% IACS at 68°F3.5(1)
Modulus of Elasticity in Tensionksi15000
Fabrication Properties
Technique Suitability
SolderingExcellent
BrazingExcellent
Oxyacetylene WeldingGood
Gas Shielded Arc WeldingExcellent
Coated Metal Arc WeldingGood
Spot WeldExcellent
Seam WeldExcellent
Butt WeldExcellent
Capacity for Being Cold WorkedGood
Capacity for Being Hot FormedGood
Machinability Rating60
Fabrication Process Properties

No fabrication process properties for this alloy

Thermal Characteristics

No thermal characteristics for this alloy

Typical uses
Product Category Product Reason Category Reason
IndustrialSheet, strip, plate, and tube
Applicable Specifications

No applicable specifications for this alloy

Corrosion Properties

No information available.