Find suppliers for this alloy
C67300
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Al | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. (3) Ni value includes Co. |
|||||||||
| Min (%) | 58.0 | 0.40 | 2.0 | 0.50 | |||||
| Max (%) | 63.0 | 3.0 | 0.30 | Rem | 0.50 | 0.25 | 0.25 | 3.5 | 1.5 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Section Size (in) |
|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||||
| Bar | Extruded and Drawn | H50 |
65 Min |
40 Min |
11 Min |
80 Min |
<1.00 |
| Melting Point - Liquidus°F | 1605 |
|---|---|
| Densitylb/cu in. at 68°F | 0.3 |
| Specific Gravity | 8.3 |
| Electrical Conductivity% IACS at 68°F | 22 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 55 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11 |
| Modulus of Elasticity in Tensionksi | 17000 |
Fabrication Properties
Common Fabrication Processes
- Hot Forming
- Hot Pressing
- Machining
Thermal Properties
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Fasteners | Fasteners | Corrosion Resistance | Corrosion Resistance |
| Fasteners | Corrosion Resistance | Stress Corrosion Cracking Resistance | |
| Fasteners | Machining Characteristics | Machinability | |
| Fasteners | Mechanical Properties | High Strength | |
| Lead Screw Nuts | Corrosion Resistance | Corrosion Resistance | |
| Lead Screw Nuts | Machining Characteristics | Machinability | |
| Lead Screw Nuts | Mechanical Properties | High Strength | |
| Industrial | Bearings | Friction & Wear Properties | Wear Resistance |
| Bearings | Machining Characteristics | Machinability | |
| Bearings | Mechanical Properties | Strength | |
| Bearings, Pins | Corrosion Resistance | Corrosion Resistance | |
| Bearings, Pins | Friction & Wear Properties | Low Co-efficient of Friction | |
| Bearings, Pins | Friction & Wear Properties | Wear Resistance | |
| Bearings, Pins | Machining Properties | Machinability, Good | |
| Bearings, Pins | Mechanical Properties | High Strength | |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Friction & Wear Properties | Galling Resistance | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Bushings | Machining Characteristics | Machinability | |
| Clutch Bearings | Corrosion Resistance | Corrosion Resistance | |
| Clutch Bearings | Friction & Wear Properties | Low Co-efficient of Friction | |
| Clutch Bearings | Friction & Wear Properties | Wear Resistance | |
| Clutch Bearings | Machining Properties | Machinability, Good | |
| Clutch Bearings | Mechanical Properties | High Strength | |
| Drive Shafts | Corrosion Resistance | Corrosion Resistance | |
| Drive Shafts | Friction & Wear Properties | Wear Resistance | |
| Drive Shafts | Mechanical Properties | Fatigue Strength | |
| Drive Shafts | Mechanical Properties | High Strength | |
| Gears and Cams | Corrosion Resistance | Corrosion Resistance | |
| Gears and Cams | Machining Characteristics | Machinability | |
| Gears and Cams | Mechanical Properties | Fatigue Resistance | |
| Gears and Cams | Mechanical Properties | High Strength | |
| Idler Pins | Corrosion Resistance | Corrosion Resistance | |
| Idler Pins | Mechanical Properties | Fatigue Strength | |
| Idler Pins | Mechanical Properties | High Strength | |
| Piston Heads | Corrosion Resistance | Corrosion Resistance | |
| Piston Heads | Friction & Wear Properties | Galling Resistance | |
| Piston Heads | Friction & Wear Properties | Wear Resistance | |
| Piston Heads | Machining Properties | Machinability, Good | |
| Piston Heads | Mechanical Properties | Fatigue Strength | |
| Piston Heads | Mechanical Properties | High Strength | |
| Propeller Shafts | Corrosion Resistance | Corrosion Resistance | |
| Propeller Shafts | Friction & Wear Properties | Galling Resistance | |
| Propeller Shafts | Friction & Wear Properties | Wear Resistance | |
| Propeller Shafts | Machining Properties | Machinability, Good | |
| Propeller Shafts | Mechanical Properties | High Strength | |
| Pump Parts | Corrosion Resistance | Corrosion Resistance | |
| Pump Parts | Friction & Wear Properties | Galling Resistance | |
| Pump Parts | Friction & Wear Properties | Wear Resistance | |
| Pump Parts | Machining Properties | Machinability, Good | |
| Pump Parts | Mechanical Properties | High Strength | |
| Seal Rings | Corrosion Resistance | Corrosion Resistance | |
| Seal Rings | Friction & Wear Properties | Galling Resistance | |
| Seal Rings | Friction & Wear Properties | Wear Resistance | |
| Seal Rings | Machining Properties | Machinability, Good | |
| Seal Rings | Mechanical Properties | Ductility | |
| Seal Rings | Mechanical Properties | High Strength | |
| Shaft Bushings | Corrosion Resistance | Corrosion Resistance | |
| Shaft Bushings | Friction & Wear Properties | Galling Resistance | |
| Shaft Bushings | Friction & Wear Properties | Low Co-efficient of Friction | |
| Shaft Bushings | Friction & Wear Properties | Wear Resistance | |
| Shaft Bushings | Machining Properties | Machinability, Good | |
| Shaft Bushings | Mechanical Properties | High Strength | |
| Sleeve Bearings | Corrosion Resistance | Corrosion Resistance | |
| Sleeve Bearings | Friction & Wear Properties | Galling Resistance | |
| Sleeve Bearings | Friction & Wear Properties | Low Co-efficient of Friction | |
| Sleeve Bearings | Friction & Wear Properties | Wear Resistance | |
| Sleeve Bearings | Machining Properties | Machinability, Good | |
| Sleeve Bearings | Mechanical Properties | High Strength | |
| Spindles | Corrosion Resistance | Corrosion Resistance | |
| Spindles | Machining Properties | Machinability, Good | |
| Spindles | Mechanical Properties | Ductility | |
| Spindles | Mechanical Properties | Fatigue Strength | |
| Spindles | Mechanical Properties | High Strength | |
| Thrust Bearings | Corrosion Resistance | Corrosion Resistance | |
| Thrust Bearings | Friction & Wear Properties | Low Co-efficient of Friction | |
| Thrust Bearings | Friction & Wear Properties | Wear Resistance | |
| Thrust Bearings | Mechanical Properties | High Strength | |
| Wear Plates | Corrosion Resistance | Corrosion Resistance | |
| Wear Plates | Friction & Wear Properties | Galling Resistance | |
| Wear Plates | Friction & Wear Properties | Wear Resistance | |
| Wear Plates | Machining Characteristics | Machinability | |
| Marine | Hardware | Corrosion Resistance | Corrosion Resistance |
| Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Hardware | Machining Characteristics | Machinability | |
| Hardware | Mechanical Properties | High Strength | |
| Valve Seats | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Valve Seats | Friction & Wear Properties | Wear Resistance | |
| Valve Seats | Mechanical Properties | Ductility | |
| Valve Seats | Mechanical Properties | High Strength | |
| Other | Connecting Rods | Corrosion Resistance | Corrosion Resistance |
| Connecting Rods | Friction & Wear Properties | Wear Resistance | |
| Connecting Rods | Machining Characteristics | Machinability | |
| Connecting Rods | Mechanical Properties | Fatigue Life | |
| Connecting Rods | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Forgings | Forgings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Forgings | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Rod | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Shapes | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS |
Corrosion Properties