Find suppliers for this alloy
C67340
| Elements | ||||||||
|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Zn | Fe | Ni(3) | Al | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.8% min. (2) Cu value includes Ag. (3) Ni value includes Co. |
||||||||
| Min (%) | 60.0 | 0.20 | 0.20 | 0.50 | 1.5 | 0.50 | ||
| Max (%) | 63.5 | 0.10 | Rem | 0.7 | 0.6 | 1.0 | 2.0 | 1.0 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.2% Offset (ksi) |
Elongation (%) |
|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). | |||||
| Rod, Bar & Wire | 1/2 Hard | H02 |
80 Typ |
65 Typ |
20 Typ |
| Hard | H04 |
94 Typ |
81 Typ |
||
| Melting Point - Liquidus°F | 1625 |
|---|---|
| Melting Point - Solidus°F | 1544 |
| Densitylb/cu in. at 68°F | 0.295 |
| Specific Gravity | 8.15 |
| Electrical Conductivity% IACS at 68°F | 19 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 520 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10.9 |
| Modulus of Elasticity in Tensionksi | 17000 |
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Fair |
| Oxyacetylene Welding | Fair |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Fair |
| Spot Weld | Fair |
| Seam Weld | Fair |
| Butt Weld | Fair |
| Capacity for Being Cold Worked | Good |
| Capacity for Being Hot Formed | Excellent |
| Machinability Rating | 70 |
Common Fabrication Processes
Thermal Properties
Typical Uses
Applicable Specifications
Corrosion Properties