C67400
| Elements | |||||||||
|---|---|---|---|---|---|---|---|---|---|
| Cu(1,2) | Pb | Sn | Zn | Fe | Ni(3) | Al | Mn | Si | |
|
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. (3) Ni value includes Co. |
|||||||||
| Min (%) | 57.0 | 0.50 | 2.0 | 0.50 | |||||
| Max (%) | 60.0 | 0.50 | 0.30 | Rem | 0.35 | 0.25 | 2.0 | 3.5 | 1.5 |
| Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Shear Strength (ksi) |
Fatigue Strength** (ksi) |
Section Size (in) |
|---|---|---|---|---|---|---|---|---|---|
| * Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||
| Bar | 1/2 Hard and Stress Relieved | HR02 |
85 Typ |
45 Typ |
24 Typ |
83 Typ |
|||
| As Hot Extruded | M30 |
78 Typ |
38 Typ |
26 Typ |
78 Typ |
||||
| Rod | 1/2 Hard and Stress Relieved | HR02 |
92 Typ |
55 Typ |
20 Typ |
87 Typ |
48 Typ |
29 Typ | 0.75 |
| Soft Anneal | O60 |
70 Typ |
34 Typ |
28 Typ |
78 Typ |
0.75 | |||
| Melting Point - Liquidus°F | 1625 |
|---|---|
| Melting Point - Solidus°F | 1590 |
| Densitylb/cu in. at 68°F | 0.292 |
| Specific Gravity | 8.08 |
| Electrical Conductivity% IACS at 68°F | 23 |
| Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 58 |
| Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 11 |
| Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
| Modulus of Elasticity in Tensionksi | 16000 |
| Modulus of Rigidityksi | 6000 |
| Technique | Suitability |
|---|---|
| Soldering | Fair |
| Brazing | Good |
| Oxyacetylene Welding | Not Recommended |
| Gas Shielded Arc Welding | Fair |
| Coated Metal Arc Welding | Not Recommended |
| Spot Weld | Good |
| Seam Weld | Good |
| Butt Weld | Good |
| Capacity for Being Cold Worked | Poor |
| Capacity for Being Hot Formed | Excellent |
| Forgeability Rating | 100 |
| Machinability Rating | 30 |
Common Fabrication Processes
- Hot Forging and Pressing
- Machining
| Treatment | Minimum* | Maximum* | ||
|---|---|---|---|---|
| * Temperature is measured in Fahrenheit. | ||||
| Annealing | 800 | 1100 | ||
| Hot Working Temperature | 1100 | 1250 | ||
| Product Category | Product | Reason Category | Reason |
|---|---|---|---|
| Industrial | Bushings | Bearing Properties | Bearing Properties Against Hardened Steel |
| Bushings | Corrosion Resistance | Corrosion Resistance | |
| Bushings | Corrosion Resistance | Corrosion Resistance to Salt Water | |
| Bushings | Friction & Wear Properties | Galling Resistance | |
| Bushings | Friction & Wear Properties | Wear Resistance | |
| Cams | Corrosion Resistance | Corrosion Resistance | |
| Cams | Friction & Wear Properties | Galling Resistance | |
| Cams | Friction & Wear Properties | Wear Resistance | |
| Cams | Mechanical Properties | High Strength | |
| Chain Guides | Corrosion Resistance | Corrosion Resistance | |
| Chain Guides | Friction & Wear Properties | Wear Resistance | |
| Chain Guides | Mechanical Properties | High Strength | |
| Food Conveyor Chain | Corrosion Resistance | Corrosion Resistance | |
| Food Conveyor Chain | Friction & Wear Properties | Wear Resistance | |
| Food Conveyor Chain | Mechanical Properties | High Strength | |
| Gears | Corrosion Resistance | Corrosion Resistance | |
| Gears | Friction & Wear Properties | Galling Resistance | |
| Gears | Friction & Wear Properties | Wear Resistance | |
| Gears | Mechanical Properties | High Strength | |
| Shafts | Corrosion Resistance | Corrosion Resistance | |
| Shafts | Friction & Wear Properties | Wear Resistance | |
| Shafts | Mechanical Properties | Fatigue Strength | |
| Shafts | Mechanical Properties | High Strength | |
| Wear Plates | Bearing Properties | Bearing Properties Against Hardened Steel | |
| Wear Plates | Corrosion Resistance | Corrosion Resistance | |
| Wear Plates | Friction & Wear Properties | Galling Resistance | |
| Wear Plates | Friction & Wear Properties | Wear Resistance | |
| Other | Connecting Rods | Corrosion Resistance | Corrosion Resistance |
| Connecting Rods | Mechanical Properties | Fatigue Life | |
| Connecting Rods | Mechanical Properties | High Strength |
| Form | Specific Sub-Form | Application | System | Standard | Description |
|---|---|---|---|---|---|
| Bar | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
| Forgings | Forgings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
| Forgings | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
| Rod | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
| Shapes | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
| SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS |
Corrosion Properties