Find suppliers for this alloyC67400
Chemical Composition
Element
Cu(1,2)PbSnZnFeNi(3)AlMnSi
(1) Cu + Sum of Named Elements 99.5% min. (2) Cu value includes Ag. (3) Ni value includes Co.
Min (%)57.00.502.00.50
Max (%)60.00.500.30Rem0.350.252.03.51.5
Mechanical Properties*
Form
Temper
Temper Code
Tensile Strength
(ksi)
YS-0.5% Ext
(ksi)
Elongation
(%)
Rockwell B scale
Shear Strength
(ksi)
Fatigue Strength**
(ksi)
Section Size
(in)
Bar1/2 Hard and Stress RelievedHR0285   Typ
45   Typ
24   Typ
83   Typ
As Hot ExtrudedM3078   Typ
38   Typ
26   Typ
78   Typ
Rod1/2 Hard and Stress RelievedHR0292   Typ
55   Typ
20   Typ
87   Typ
48   Typ
29   Typ
0.75
Soft AnnealO6070   Typ
34   Typ
28   Typ
78   Typ
0.75
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106.
Physical Properties
Melting Point - Liquidus°F1625
Melting Point - Solidus°F1590
Densitylb/cu in. at 68°F0.292
Specific Gravity8.08
Electrical Conductivity% IACS at 68°F23
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F58
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F)11
Specific Heat CapacityBtu/ lb /°F at 68°F0.09
Modulus of Elasticity in Tensionksi16000
Modulus of Rigidityksi6000
Fabrication Properties
Technique Suitability
SolderingFair
BrazingGood
Oxyacetylene WeldingNot Recommended
Gas Shielded Arc WeldingFair
Coated Metal Arc WeldingNot Recommended
Spot WeldGood
Seam WeldGood
Butt WeldGood
Capacity for Being Cold WorkedPoor
Capacity for Being Hot FormedExcellent
Forgeability Rating100
Machinability Rating30
Common Fabrication Processes
  • Hot Forging and Pressing
  • Machining
    
Thermal Properties
Treatment Minimum* Maximum*
* Temperature is measured in Fahrenheit.
Annealing8001100
Hot Treatment11001250
Typical uses
Product Category Product Reason Category Reason
IndustrialBushingsBearing PropertiesBearing Properties Against Hardened Steel
BushingsCorrosion ResistanceCorrosion Resistance
BushingsCorrosion ResistanceCorrosion Resistance to Salt Water
BushingsFriction & Wear PropertiesGalling Resistance
BushingsFriction & Wear PropertiesWear Resistance
CamsCorrosion ResistanceCorrosion Resistance
CamsFriction & Wear PropertiesGalling Resistance
CamsFriction & Wear PropertiesWear Resistance
CamsMechanical PropertiesHigh Strength
Chain GuidesCorrosion ResistanceCorrosion Resistance
Chain GuidesFriction & Wear PropertiesWear Resistance
Chain GuidesMechanical PropertiesHigh Strength
Food Conveyor ChainCorrosion ResistanceCorrosion Resistance
Food Conveyor ChainFriction & Wear PropertiesWear Resistance
Food Conveyor ChainMechanical PropertiesHigh Strength
GearsCorrosion ResistanceCorrosion Resistance
GearsFriction & Wear PropertiesGalling Resistance
GearsFriction & Wear PropertiesWear Resistance
GearsMechanical PropertiesHigh Strength
ShaftsCorrosion ResistanceCorrosion Resistance
ShaftsFriction & Wear PropertiesWear Resistance
ShaftsMechanical PropertiesFatigue Strength
ShaftsMechanical PropertiesHigh Strength
Wear PlatesBearing PropertiesBearing Properties Against Hardened Steel
Wear PlatesCorrosion ResistanceCorrosion Resistance
Wear PlatesFriction & Wear PropertiesGalling Resistance
Wear PlatesFriction & Wear PropertiesWear Resistance
OtherConnecting RodsCorrosion ResistanceCorrosion Resistance
Connecting RodsMechanical PropertiesFatigue Life
Connecting RodsMechanical PropertiesHigh Strength
Applicable Specifications
Form Sub-Form System Standard Description
BarSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ForgingsForgingsSAEJ461WROUGHT AND CAST COPPER ALLOYS
ForgingsSAEJ463WROUGHT COPPER AND COPPER ALLOYS
RodSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
ShapesSAEJ461WROUGHT AND CAST COPPER ALLOYS
SAEJ463WROUGHT COPPER AND COPPER ALLOYS
Corrosion Properties

No information available.